Preparation method and application of nano composite hydrogel
By preparing nanocomposite hydrogels of calcium phosphotungate sub-nanowires and PVA, the dual network structure is used to improve the mechanical properties, and the problem of insufficient mechanical properties of materials in the prior art is solved, and the nanocomposite water with high modulus and toughness is achieved Gel, suitable for wearable electronic devices and software robots.
Patent Information
- Application Number
- CN202411239701.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The existing inorganic sub-nanowire/PDMS composite elastomer materials have low elongation at break and cannot meet the requirements of high mechanical properties in some application fields, such as material requirements in wearable sensors and soft robots.
By preparing calcium phosphotungstenate sub-nanowires combined with polyvinyl alcohol (PVA), calcium phosphotungstenate sub-nanowires/PVA nanocomposite hydrogels are formed, and the hydrogen bond interaction between inorganic sub-nanowires and PVA is constructed by constructing double-tongues Network structure to improve the mechanical properties of hydrogels.
The high modulus and toughness of nanocomposite hydrogels have been achieved, with a fracture stress of 0.8MPa and an elongation of break of 650%, which has greatly improved its application potential in the fields of wearable electronic devices and software robots.
Smart Images

Figure CN119060367A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-performance and functional nanocomposite hydrogels, and in particular to a preparation method of a nanocomposite hydrogel and an application thereof. Background Art
[0002] Nanocomposite hydrogel refers to a composite hydrogel constructed by adding fillers such as organic / inorganic nanoparticles and nanowires to a soft hydrogel matrix. The addition of nanofillers can make the hydrogel have good mechanical properties. Its enhancement mechanism is mainly attributed to two aspects: first, the interaction between fillers and polymers can increase the cross-linking degree of the gel network; second, the fillers can bear part of the load and disperse the deformation force of the gel.
[0003] The type of hydrogel matrix and the type of added fillers such as nanoparticles and nanowires have a huge impact on the mechanical properties of composite hydrogels. Different application fields have different requirements for the mechanical properties of nanocomposite hydrogels. Therefore, in order to expand the application fields of nanocomposite hydrogels, it is of great significance to develop composite hydrogels with excellent mechanical properties.
[0004] "A method for preparing an inorganic sub-nanowire / PDMS composite elastomer material" (patent application number: 202311334895.8). This technology forms an organic gel by self-assembly of inorganic sub-nanowires and organic matter (such as octane and cyclohexane), and then composites PDMS and inorganic sub-nanowire organic gel to obtain a new type of composite material. PDMS (polydimethylsiloxane) can be directly used for moisture-proof insulation, damping, shock absorption, etc., and is widely used as insulating lubrication, shockproof, and heat carrier. The elongation at break of the inorganic sub-nanowire / PDMS composite elastomer material prepared by the method is relatively low, with a maximum of less than 10%. The application field of organic gels with such mechanical properties is still very limited. For example, materials that can be widely used in wearable sensors, soft robots, medical materials and other fields generally require the elongation at break of the gel to be above 200%. The organic gel prepared by patent 202311334895.8 cannot meet the requirements at all.
[0005] Therefore, developing a composite hydrogel with excellent mechanical properties and further expanding its application range is a technical problem that needs to be solved urgently. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a nano composite hydrogel. The preparation method is simple, and the prepared hydrogel has high modulus and toughness and excellent mechanical properties.
[0007] To achieve the above object, the present invention provides a method for preparing a nanocomposite hydrogel, comprising the following steps:
[0008] (1) preparing calcium phosphotungstate sub-nanowires;
[0009] (2) dispersing PVA in a mixed solution of water and ethylene glycol to obtain a PVA dispersion;
[0010] (3) adding the sub-nanowires prepared in step (1) to the PVA dispersion in step (2), and then subjecting the mixture to a gelling treatment to obtain a calcium phosphotungstate sub-nanowire / PVA nanocomposite hydrogel.
[0011] Furthermore, the specific steps of preparing calcium phosphotungstate sub-nanowires in step (1) are as follows:
[0012] 0.5-2g of phosphotungstic acid hydrate, 0.06-0.26g of calcium nitrate tetrahydrate and 8-32mL of deionized water were mixed, and stirred at a speed of 300-500rpm / min for 10 minutes to obtain a clear solution; 6-24mL of 1-octadecene and 2-8mL of oleylamine were added in sequence, and then stirred at a speed of 200-400rpm / min for 8 hours to obtain a white viscous liquid. The reaction product was poured into a centrifuge tube, and 20-30mL of cyclohexane and ethanol were added respectively for centrifugal washing for 3-5 times to obtain calcium phosphotungstate sub-nanowires; the centrifugal speed was 8000-10000rpm / min, and the centrifugal time was 5min.
[0013] Furthermore, the diameter of the calcium phosphotungstate sub-nanowires prepared in step (1) is 0.8 to 1.2 nm.
[0014] Furthermore, in step (2), the mass ratio of water to ethylene glycol is 2:1, and the mass ratio of PVA to the mixed solution of water and ethylene glycol is 1:10.
[0015] Furthermore, in the step (3), the mass ratio of calcium phosphotungstate sub-nanowires to the PVA dispersion is 1:20 to 1:100.
[0016] Furthermore, the gelling treatment in step (3) is carried out under the conditions of placing the mixed solution at -15 to -20°C for 20 to 24 hours, and then taking it out and placing it at room temperature for 2 to 3 hours.
[0017] The present invention also provides an application of the nanocomposite hydrogel prepared by the preparation method as described above in wearable electronic devices, tissue engineering, and soft robots.
[0018] The nanocomposite hydrogel of the present invention has excellent mechanical properties due to the introduction of sub-nanowires on the basis of the biocompatibility of PVA, and therefore has good application prospects in the fields of wearable electronic devices, tissue engineering, soft robots, etc.
[0019] Compared with the prior art, the advantages and positive effects of the present invention are:
[0020] 1. The preparation process of the present invention is simple and easy.
[0021] 2. Compared with pure PVA hydrogel, the nanocomposite hydrogel prepared by the present invention has higher modulus and toughness, excellent mechanical properties, and has wide applicability and promotion value.
[0022] The network structure formed by polyvinyl alcohol in the nanocomposite hydrogel serves as the matrix structure of the hydrogel, providing basic mechanical properties for the hydrogel. Inorganic sub-nanowires are used as a nano-enhanced filler to construct a double network hydrogel together with PVA due to their good flexibility and large aspect ratio. A large number of hydrogen bonds can be formed between inorganic sub-nanowires, PVA and ethylene glycol, so that there is a strong interaction between the inorganic sub-nanowire network and the PVA network, so that the formed double network hydrogel has excellent mechanical properties. With the increase of sub-nanowire content, the interaction between the inorganic sub-nanowire network and the PVA network is also enhanced, and then the mechanical properties of the sub-nanowire / PVA nanocomposite hydrogel are gradually increased. Among them, the fracture stress of PVA / Ca-POM5 reaches 0.8MPa and the elongation at break reaches 650%, which is at a relatively high level in the fields of wearable electronic devices, soft robots, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a TEM image of the inorganic sub-nanowire of calcium phosphotungstate prepared in Example 1;
[0024] Figure 2 The tensile stress-strain curve comparison diagram of the hydrogels prepared in Examples 1, 2, 3, and 4;
[0025] Figure 3 The figure is a comparison chart of the modulus and toughness of the hydrogels prepared in Examples 1, 2, 3, and 4. DETAILED DESCRIPTION
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0027] The technical solution of the present invention is further explained below in conjunction with implementation cases.
[0028] Example 1
[0029] This embodiment provides a method for preparing a nanocomposite hydrogel, and the specific preparation steps are as follows:
[0030] S1, preparing calcium phosphotungstate sub-nanowires;
[0031] S1-1, 1.0 g of phosphotungstic acid hydrate, 0.123 g of calcium nitrate hydrate and 16 mL of deionized water were mixed and stirred into a clear solution, and then 12 mL of 1-octadecene and 4 mL of oleylamine were added in sequence, and stirred at room temperature and a speed of 300 rpm / min for 8 hours to obtain a white viscous liquid;
[0032] S1-2, pour the reaction product into a centrifuge tube, add 25mL cyclohexane and ethanol respectively, and centrifuge and wash three times to obtain calcium phosphotungstate sub-nanowires (Ca-POM). The centrifugal speed is 10000rpm / min, the centrifugal time is 5min, and the product obtained by centrifugation contains a small amount of cyclohexane and ethanol, and is in a semi-solid state.
[0033] S2. Dispersing PVA in a mixed solution of water and ethylene glycol to obtain a PVA dispersion, wherein the mass ratio of water to ethylene glycol is 2:1, and the mass ratio of PVA to the mixed solution of water and ethylene glycol is 1:10.
[0034] S3. Adding the prepared sub-nanowires into the PVA dispersion to obtain a mixed solution with a certain viscosity, wherein the mass ratio of the sub-nanowires to the PVA dispersion is 1:100.
[0035] S4. The obtained mixed solution with a certain viscosity was placed at -20°C for 24 hours, and then taken out and placed at room temperature for 2 hours to obtain a sub-nanowire / PVA nanocomposite hydrogel, which was named PVA / Ca-POM1.
[0036] Example 2
[0037] This embodiment provides a method for preparing a nanocomposite hydrogel. The specific preparation steps refer to Example 1. The difference from Example 1 is that the mass ratio of the sub-nanowire to the PVA dispersion in this embodiment is 1:40. The obtained sub-nanowire / PVA nanocomposite hydrogel is named PVA / Ca-POM 2.5 .
[0038] Example 3
[0039] This embodiment provides a method for preparing a nanocomposite hydrogel. The specific preparation steps refer to Example 1. The difference from Example 1 is that the mass ratio of sub-nanowires to PVA dispersion in this embodiment is 1:20. The obtained sub-nanowire / PVA nanocomposite hydrogel is named PVA / Ca-POM5.
[0040] Example 4
[0041] This embodiment provides a method for preparing a PVA hydrogel, and the specific preparation steps are as follows:
[0042] S1. Dispersing PVA in a mixed solution of water and ethylene glycol to obtain a PVA dispersion, wherein the mass ratio of water to ethylene glycol is 2:1, and the mass ratio of PVA to the mixed solution of water and ethylene glycol is 1:10.
[0043] S2. Place the PVA dispersion at -20°C for 24 hours, then take it out and place it at room temperature for 2 hours to obtain a PVA hydrogel, which is named PVA.
[0044] Performance Test:
[0045] TEM image of the inorganic sub-nanowires prepared in Example 1, Figure 1 It can be seen that the inorganic sub-nanowires were successfully prepared, and the sub-nanowires were arranged in a linear shape with a diameter of about 1nm. The characteristic size of the sub-nanowires is close to the diameter of the polymer chain / DNA single chain, has good flexibility and a large aspect ratio, and exhibits polymer-like properties. Therefore, it can be used as a nanofiller to self-assemble with PVA to construct a nanocomposite hydrogel material.
[0046] The tensile properties of the hydrogels prepared in Examples 1-4 of the present invention were tested respectively. A hydrogel with a thickness of 2 mm and a rectangular shape (length 50 mm, width 10 mm) was prepared, and the tensile properties of the hydrogel were tested at room temperature using a domestic SHIMADZU universal testing machine. During the test, the sample was stretched at a speed of 20 mm / min. The test results are shown in FIG. Figure 2 As shown, the stress-strain curve of the hydrogel is obtained. The stress-strain curve is integrated to obtain the toughness data of the material. The slope of the stress-strain curve within the strain range of 10 to 20% is used to represent the Young's modulus of the material. The results are shown in Figure 3 As shown in the figure, the modulus and toughness comparison of the hydrogel is obtained. Figure 2 , 3 It can be seen that the nanocomposite hydrogel has higher modulus and toughness than pure PVA hydrogel, and has excellent mechanical properties. With the increase of sub-nanowire content, the interaction between the inorganic sub-nanowire network and the PVA network is also enhanced, and then the mechanical properties of the sub-nanowire / PVA nanocomposite hydrogel gradually increase. Among them, the fracture stress of PVA / Ca-POM5 reaches 0.8MPa and the elongation at break reaches 650%, which is at a relatively high level in the fields of wearable electronic devices, soft robots, etc.
[0047] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a nanocomposite hydrogel, characterized in that: The following steps are involved: (1) preparing calcium phosphotungstate sub-nanowires; (2) dispersing PVA in a mixed solution of water and ethylene glycol to obtain a PVA dispersion; (3) adding the sub-nanowires prepared in step (1) to the PVA dispersion in step (2), and then subjecting the mixture to a gelling treatment to obtain a calcium phosphotungstate sub-nanowire / PVA nanocomposite hydrogel.
2. The method for preparing a nanocomposite hydrogel according to claim 1, characterized in that: The specific steps of preparing calcium phosphotungstate sub-nanowires in step (1) are as follows: 0.5-2g of phosphotungstic acid hydrate, 0.06-0.26g of calcium nitrate tetrahydrate and 8-32mL of deionized water were mixed, and stirred at a speed of 300-500rpm / min for 10 minutes to obtain a clear solution; 6-24mL of 1-octadecene and 2-8mL of oleylamine were added in sequence, and then stirred at a speed of 200-400rpm / min for 8 hours to obtain a white viscous liquid. The reaction product was poured into a centrifuge tube, and 20-30mL of cyclohexane and ethanol were added respectively for centrifugal washing for 3-5 times to obtain calcium phosphotungstate sub-nanowires; the centrifugal speed was 8000-10000rpm / min, and the centrifugal time was 5min.
3. The method for preparing a nanocomposite hydrogel according to claim 1, characterized in that: The diameter of the calcium phosphotungstate sub-nanowires prepared in the step (1) is 0.8-1.2 nm.
4. The method for preparing a nanocomposite hydrogel according to claim 1, characterized in that: In the step (2), the mass ratio of water to ethylene glycol is 2:1, and the mass ratio of PVA to the mixed solution of water and ethylene glycol is 1:
10.
5. The method for preparing a nanocomposite hydrogel according to claim 1, characterized in that: In the step (3), the mass ratio of calcium phosphotungstate sub-nanowires to PVA dispersion is 1:20 to 1:
100.
6. The method for preparing a nanocomposite hydrogel according to claim 1, characterized in that: The gelling treatment in step (3) is performed by placing the mixed solution at -15 to -20°C for 20 to 24 hours, then taking it out and placing it at room temperature for 2 to 3 hours.
7. Application of the nanocomposite hydrogel prepared by the preparation method according to any one of claims 1 to 6 in wearable electronic devices, tissue engineering, and soft robots.
Citation Information
Patent Citations
PVA (polyvinyl alcohol) composite aquagel with bioactivity and preparation method thereof
CN102634042A
Sub-nanowire adhesive as well as preparation method and application thereof
CN113402988A
Flexible composite conductive hydrogel as well as preparation method and application thereof
CN115926201A
Preparation method of inorganic sub-nanowire / tert-butyl acrylate composite elastomer material
CN117209649A
Preparation method of inorganic sub-nanowire / PDMS composite elastomer material
CN117264242A
Cited By
PVDF (Polyvinylidene Fluoride) / Ca-POM (Polyoxymethylene) composite fiber membrane, preparation method thereof and application of PVDF / Ca-POM composite fiber membrane in preparation of wearable flexible piezoelectric sensor
CN119615497A