Preparation process of chemical-resistant and high-thermal-conductivity polyethylene pipe material for energy storage

Chemical-resistant and highly thermally conductive polyethylene tube materials were prepared by surface treatment of carbon nanotubes and polyethylene cross-linking reactions, which solved the problem of insufficient thermal conductivity and chemical resistance of polyethylene materials, and achieved efficient heat dissipation and resistance. Corrosive, suitable for the application of liquid flow energy storage technology.

CN119060370APending Publication Date: 2024-12-03SUQIAN TIMES ENERGY STORAGE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411351787.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing polyethylene materials have poor thermal conductivity, which is difficult to meet the heat dissipation needs of high-efficiency energy storage equipment. At the same time, there are also shortcomings in chemical resistance, which is difficult to meet the application requirements of liquid flow energy storage technology.

Method used

By performing specific surface treatment on carbon nanotubes, its dispersion is improved, and cross-linking is carried out with polyethylene to form a three-dimensional mesh structure, and carbon nanotubes are fixed to improve thermal conductivity and corrosion resistance. A twin-screw extrusion mechanism is used to prepare Chemical resistant, highly thermally conductive polyethylene pipe material.

Benefits of technology

The thermal conductivity and chemical resistance of the material are significantly improved, making it suitable for heat dissipation structural parts of energy storage equipment, meeting the application needs of liquid flow energy storage technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer composite materials, and discloses a preparation process of a chemical-resistant and high-thermal-conductivity polyethylene pipe material for energy storage. Specific surface treatment is carried out on the carbon nanotubes, the surface polarity of the carbon nanotubes is improved, agglomeration of powder is reduced, the dispersity of the carbon nanotubes in the material is improved, meanwhile, peroxide is used for carrying out cross-linking reaction on the polyethylene material, polyethylene molecular chains form a three-dimensional network structure, the carbon nanotubes are fixed, and a heat conduction path is formed; the overall corrosion resistance of the material is improved while the heat conductivity coefficient of the material is increased; the heat-conducting polyethylene material disclosed by the invention can be used as a heat dissipation structural member in an energy storage overall scheme.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer composite materials, and in particular relates to a preparation process of a novel chemical-resistant and high-thermal-conductivity polyethylene pipe material for energy storage. Background Art

[0002] Liquid flow energy storage is an emerging large-scale energy storage technology with broad application prospects and important strategic significance. With the transformation of the global energy structure, the proportion of renewable energy such as solar energy and wind energy continues to increase. These energy sources are intermittent and unstable, resulting in large fluctuations in power supply. In order to effectively integrate renewable energy and achieve stable supply and efficient use of electricity, the demand for large-scale energy storage technology is becoming increasingly urgent. Liquid flow energy storage technology came into being in this context. Its working principle is to convert electrical energy into chemical energy for storage through redox reaction, and then convert chemical energy into electrical energy for release when needed. Compared with traditional energy storage technology, liquid flow energy storage has many advantages. First, its energy storage capacity and power can be designed independently, which is convenient for flexible adjustment according to actual needs. Secondly, the cycle life of liquid flow batteries is long and can be charged and discharged for tens of thousands of times. Furthermore, since the electrolyte can be stored in an external storage tank, the maintenance and update of the system is relatively easy and safe.

[0003] In practical applications, liquid flow energy storage technology has shown great potential in the fields of renewable energy integration, grid peak regulation, distributed energy systems, etc. In the future, with the continuous advancement of technology and the reduction of costs, liquid flow energy storage is expected to play a more important role in the energy field and promote global energy transformation and sustainable development.

[0004] Polyethylene (PE) is one of the five major synthetic resins, with the advantages of good chemical stability, resistance to most acids and alkalis (not resistant to oxidizing acids), insoluble in general solvents at room temperature, low water absorption, and excellent electrical insulation. However, the thermal conductivity of ordinary polyethylene is relatively poor. In order to improve the thermal conductivity of polyethylene, thermal conductive polyethylene materials can be prepared by adding some thermal conductive fillers. For example, some studies have used coupling agents and grinding disc-type mechanochemical reactors to surface treat graphite, and then filled it into high-density polyethylene (HDPE). The thermal conductivity of the resulting HDPE / graphite composite material has been improved; there are also patents that mention adding aluminum powder as a filler to polyethylene, and combining it with titanate coupling agents, dispersing lubricants, ultraviolet light absorbers, light stabilizers, antioxidants and colorants, etc., through a specific preparation method (first dry-mixing various raw materials in a high-speed mixer for 3-5 minutes, and then placing them in a twin-screw extruder for melt extrusion, cooling, pelletizing, and packaging the finished product. The temperature, residence time, and pressure of each area of ​​the twin-screw extruder have specific requirements), a polyethylene material with thermal conductivity and excellent corrosion resistance can be obtained.

[0005] In addition, thermally conductive composite materials can also be prepared by melt blending with high-density polyethylene and polypropylene as matrix materials and carbon nanotubes and boron nitride particles as thermally conductive fillers. Studies have shown that when the mass ratio of carbon nanotubes to boron nitride is 7:3, the thermal conductivity of the composite material is relatively high. These thermally conductive polyethylene materials have application potential in some specific fields. For example, they can replace traditional metal thermal conductive materials in environments that require good thermal conductivity and corrosion resistance. However, specific applications still need to be comprehensively considered based on factors such as material performance, cost, and actual needs. Summary of the invention

[0006] In order to solve the above problems, the present invention discloses a preparation process of a novel chemical-resistant and high thermal conductivity polyethylene tube material for energy storage. The present invention performs a specific surface treatment on carbon nanotubes (CNTs) to improve the surface polarity of the carbon tubes so that the powders are less likely to agglomerate and the dispersion in the material is increased. At the same time, the polyethylene material is cross-linked with peroxide to form a three-dimensional network structure of polyethylene molecular chains, fix the carbon nanotubes and form a thermal conduction path, thereby increasing the thermal conductivity of the material and improving the overall corrosion resistance of the material. The thermally conductive polyethylene material of the present invention can be used as a heat dissipation structural component in the overall energy storage solution.

[0007] To achieve the above object, the technical solution of the present invention is as follows: The present invention provides a preparation process of a novel chemical-resistant and high-thermal-conductivity polyethylene pipe material for energy storage, comprising the following steps: (1) Weigh a certain weight of polyethylene wax, coupling agent, and carbon nanotube particles, use a high-speed mixer to stir at 60°C for 10 min, and then use a twin-screw extruder to granulate to obtain prefabricated carbon nanotube masterbatch, which is then dried at 100°C for 2 h for later use.

[0008] (2) The carbon tube masterbatch, polyethylene (PE) and peroxide obtained in step (1) are mixed in a high-speed mixer for 5 minutes and then subjected to twin-screw granulation to obtain a chemically resistant and highly thermally conductive polyethylene material.

[0009] Furthermore, in step (1) and step (2), the length-to-diameter ratio of the twin-screw extruder is 48:1-60:1, and the temperature of each zone from the feeding section to the die opening is controlled to be between 160°C and 210°C.

[0010] The present invention also provides a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage prepared by the above-mentioned preparation process, comprising the following components and weight parts: 100 parts of PE, the polyethylene melt index is 3-5g / 10min; 5-10 parts of polyethylene wax, wherein the molecular weight of the polyethylene wax is 3000-5000 Daltons; 1-3 parts of coupling agent, wherein the coupling agent is one of KH550, KH560 and KH570; 1-5 parts of carbon nanotube particles, wherein the carbon nanotube particles are carbon nanotubes with a diameter of 10-20 nm, pressed into particles with a diameter of 2-3 mm and a length of 5-8 mm.

[0011] 0.01-0.1 parts of peroxide, wherein the peroxide is dicumyl peroxide (DCP).

[0012] Furthermore, in step (1), the obtained carbon nanotube masterbatch has a particle size of 3-5 mm in diameter and 5-8 mm in length.

[0013] The beneficial effects of the present invention are: In view of the drawbacks of carbon nanotubes such as agglomeration and poor dispersion that are often encountered in the application of carbon nanotubes in the plastics industry, the polyethylene / carbon nanotube composite material prepared by the above method can improve the thermal conductivity and chemical resistance of the material compared with the traditional process when the carbon nanotube content is the same, so that the material can be applied to the energy storage industry. DETAILED DESCRIPTION

[0014] The present invention will be further explained below in conjunction with specific implementation modes. It should be understood that the following specific implementation modes are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0015] Carbon nanotube particles: Carbon nanotubes with a diameter of 10-20nm are pressed into particles with a diameter of 2-3mm and a length of 5-8mm. Example 1

[0016] (1) 10kg polyethylene wax, 3kg carbon nanotube particles, and 0.2kg KH570 were mixed evenly in a high-speed mixer and fed from the main feed port. After granulation, carbon nanotube masterbatch was obtained. The extruder screw diameter was 50mm and the aspect ratio was 60:1. The temperature of each section of the extruder was set as follows (from the main feed port to the die): 210℃, 230℃, 240℃, 240℃, 250℃, 250℃, 250℃, 250℃, 250℃, 250℃, 260℃. The screw speed was 600rpm and the feed speed was 120rpm. The particle size of the carbon nanotube masterbatch was 3-5mm in diameter and 5-8mm in length.

[0017] (2) 85 kg of polyethylene, 13.2 kg of carbon nanotube masterbatch and 100 g of peroxide DCP were mixed and extruded into pellets using the same extrusion equipment and extrusion conditions. Example 2

[0018] (1) 10kg polyethylene wax, 5kg carbon nanotube particles and 0.2kg KH570 were mixed evenly in a high-speed mixer and discharged from the main feed port. After granulation, carbon nanotube masterbatch was obtained. The extruder screw diameter was 50mm and the aspect ratio was 60:1. The temperature of each section of the extruder was set as follows (from the main feed port to the die): 210℃, 230℃, 240℃, 240℃, 250℃, 250℃, 250℃, 250℃, 250℃, 250℃, 260℃. The screw speed was 600rpm and the feed speed was 120rpm. The particle size of the carbon nanotube masterbatch was 3-5mm in diameter and 5-8mm in length.

[0019] (2) 85 kg of polyethylene, 15.2 kg of carbon nanotube masterbatch and 100 g of peroxide DCP were mixed and extruded into pellets using the same extrusion equipment and extrusion conditions. Example 3

[0020] (1) 10kg polyethylene wax, 7kg carbon nanotube particles and 0.2kg KH570 were mixed evenly in a high-speed mixer and fed from the main feed port. After granulation, carbon nanotube masterbatch was obtained. The extruder screw diameter was 50mm and the aspect ratio was 60:1. The temperature of each section of the extruder was set as follows (from the main feed port to the die): 210℃, 230℃, 240℃, 240℃, 250℃, 250℃, 250℃, 250℃, 250℃, 250℃, 260℃. The screw speed was 600rpm and the feed speed was 120rpm. The particle size of the carbon nanotube masterbatch was 3-5mm in diameter and 5-8mm in length.

[0021] (2) 85 kg of polyethylene, 17.2 kg of carbon nanotube masterbatch and 100 g of peroxide DCP were mixed and extruded into pellets using the same extrusion equipment and extrusion conditions. Example 4

[0022] (1) 10kg polyethylene wax and 7kg carbon nanotube particles were mixed evenly in a high-speed mixer and discharged from the main feed port. After granulation, carbon nanotube masterbatch was obtained. The extruder screw diameter was 50mm and the aspect ratio was 60:1. The temperature of each section of the extruder was set as follows (from the main feed port to the die): 210℃, 230℃, 240℃, 240℃, 250℃, 250℃, 250℃, 250℃, 250℃, 250℃, 260℃. The screw speed was 600rpm and the feed speed was 120rpm. The particle size of the carbon nanotube masterbatch was 3-5mm in diameter and 5-8mm in length.

[0023] (2) 85 kg of polyethylene, 17 kg of carbon nanotube masterbatch and 100 g of peroxide DCP were mixed and extruded into pellets using the same extrusion equipment and extrusion conditions. Example 5

[0024] (1) 10kg polyethylene wax, 7kg carbon nanotube particles and 0.2kg KH570 were mixed evenly in a high-speed mixer and fed from the main feed port. After granulation, carbon nanotube masterbatch was obtained. The extruder screw diameter was 50mm and the aspect ratio was 60:1. The temperature of each section of the extruder was set as follows (from the main feed port to the die): 210℃, 230℃, 240℃, 240℃, 250℃, 250℃, 250℃, 250℃, 250℃, 250℃, 260℃. The screw speed was 600rpm and the feed speed was 120rpm. The particle size of the carbon nanotube masterbatch was 3-5mm in diameter and 5-8mm in length.

[0025] (2) 85 kg of polyethylene and 17.2 kg of carbon nanotube masterbatch were mixed and extruded into pellets using the same extrusion equipment and extrusion conditions.

[0026] The composite material injection molded specimens obtained above were subjected to chemical resistance test (test method see Table 1 Notes). The test results (see Table 1) show that the chemical resistance and thermal conductivity of the material produced by this patented method are significantly higher than those of the blank control sample: Table 1 Chemical resistance test data

[0027] It should be noted that the above content only illustrates the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.

Claims

1. A process for preparing a chemical-resistant and highly thermally conductive polyethylene material for energy storage, characterized in that: The following steps are involved: Add polyethylene wax, coupling agent and carbon nanotube particles into a high-speed mixer, stir at 60°C for 10 minutes, and then use a twin-screw extruder to granulate to obtain carbon nanotube masterbatch, dry at 100°C for 2 hours, and set aside; The carbon nanotube masterbatch obtained in step (1), polyethylene, and diisopropylbenzene peroxide were placed in a high-speed mixer and mixed for 5 minutes, and then pelletized using a twin-screw extruder to obtain a chemically resistant and highly thermally conductive polyethylene material.

2. The preparation process of a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage according to claim 1, characterized in that: In step (1) and step (2), the aspect ratio of the twin-screw extruder is 48:1-60:1, and the temperature of each zone from the feeding section to the die is controlled to be 160°C-210°C.

3. The preparation process of a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage according to claim 1, characterized in that: In step (1) and step (2), by weight, polyethylene is 100 parts, polyethylene wax is 5-10 parts, coupling agent is 1-3 parts, carbon nanotubes are 1-5 parts, and dicumyl peroxide is 0.01-0.1 parts.

4. The preparation process of a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage according to claim 1, characterized in that: In step (1), the molecular weight of the polyethylene wax is 3000-5000 Daltons.

5. The preparation process of a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage according to claim 1, characterized in that: In step (1), the coupling agent is one of KH550, KH560 and KH570.

6. The preparation process of a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage according to claim 1, characterized in that: In step (1), the carbon nanotube particles are made of carbon nanotubes with a diameter of 10-20 nm, which are pressed into particles with a diameter of 2-3 mm and a length of 5-8 mm.

7. The preparation process of a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage according to claim 1, characterized in that: In step (2), the melt index of polyethylene is 3-5 g / 10 min.

8. The preparation process of a novel chemical-resistant and high thermal conductivity polyethylene material for energy storage according to claim 1, characterized in that: In step (1), the obtained carbon nanotube masterbatch has a particle size of 3-5 mm in diameter and 5-8 mm in length.

9. A novel chemical-resistant and high thermal conductivity polyethylene material for energy storage prepared by the preparation process according to any one of claims 1 to 8.