Optically-driven piezoresistive sensing integrated (PVA) PNIPAM / PANI composite hydrogel material and preparation method thereof

By preparing optically driven integrated piezoresistive sensing (PVA) PNIPAM/PANI composite hydrogel material, the complexity and inefficiency of traditional drivers are solved, and high-efficiency light drive and self-perception functions are realized, suitable for inadequate lighting. In the environment.

CN119060374APending Publication Date: 2024-12-03ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410987192.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The drive performance and process of traditional soft drives are complex and inefficient, especially in the event of insufficient lighting, and are difficult to achieve integration of sensing functions for automatic control.

Method used

Using photo-driven integrated piezoresistive sensing (PVA) PNIPAM/PANI composite hydrogel material, it forms a high sensitivity and mechanical properties by configuring ammonium persulfate solution, hydrogel precursor injection molding and ultraviolet light irradiation crosslinking. Compound hydrogel uses the photothermal effect of polyaniline to achieve light-driven and self-perception functions.

Benefits of technology

It realizes rapid bending and recovery under ultraviolet light, has high sensitivity and stability, and can feedback the bending angle and rate in real time through the piezoresistive sensing layer, real-time, remote control and self-perception of the hydrogel system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060374A_ABST
    Figure CN119060374A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a light-driven integrated piezoresistive sensing composite hydrogel material, which comprises the following steps: embedding an aniline monomer, an oxidizing agent and hydrochloric acid in hydrogel in advance, carrying out hydrogel photopolymerization at 0 DEG C, and polymerizing aniline at low temperature to obtain the composite hydrogel. The composite hydrogel material prepared by the invention has excellent mechanical property, driving property and sensing property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of light-driven hydrogel preparation, and in particular relates to the preparation and application of a highly efficient light-driven integrated piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material. Background Art

[0002] Biological systems have evolved a variety of complex regulatory mechanisms to sense and respond to changes in the external environment. In the case of pine cones, due to the hygroscopic properties of individual cone scales, they can open when dry to release seeds and close when wet. Mimosa pudica is able to change the orientation of its leaves in response to mechanical stimulation (touch). Cephalopods (such as octopuses) exhibit a distributed sensory neuromotor control system with non-segmented arms that can sense their own movements (proprioception) and external tactile stimuli. The ability of these organisms to sense external stimuli and manage their movements to adapt to the environment has inspired the next paradigm of biological sensing and actuation devices. However, mimicking this biological somatosensory system to achieve active movement and perception functions requires the integration of sensors and actuators.

[0003] At present, the driving performance and process of traditional soft actuators can only be obtained through camera systems and image processing technology, which is complicated, inefficient, and not suitable for low-light conditions. Integrating the sensing function into the soft actuator can accurately obtain the deformation degree of the actuator and automatically control the actuator according to the real-time feedback signal. However, in order to meet the mechanical properties and fast driving performance required by the soft actuator in practical applications, the material composition and preparation method of the driving sensing composite hydrogel still need to be studied. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a (PVA) PNIPAM / PANI composite hydrogel material with light-driven integrated piezoresistive sensing, the method comprising the following steps:

[0005] (1) preparing an ammonium persulfate solution (APS solution): adding ammonium persulfate to deionized water and stirring until completely dissolved, then adding deionized water to prepare the solution into an ammonium persulfate solution, and then precooling for use;

[0006] (2) preparing a hydrogel precursor solution: adding a crosslinker, N-isopropylacrylamide (NIPAM), and a photoinitiator to a co-solvent and stirring the mixture to obtain a clear and transparent solution; then sequentially adding ANI, HCl solution, and PVA solution in an ice water bath; after all components are completely dissolved, adding a pre-cooled APS solution and stirring the mixture to obtain a hydrogel precursor solution;

[0007] (3) Injection molding: Inject the prepared hydrogel precursor solution into the mold, and avoid generating bubbles during the injection process;

[0008] (4) Cross-linking: The mold after injection molding is placed in an ice water bath under ultraviolet light for light curing to obtain (PVA) / PNIPAM composite hydrogel;

[0009] (5) Polymerization: The mold is then placed at low temperature to polymerize aniline. After the reaction is completed, the mold is removed and repeatedly rinsed with deionized water to obtain a light-driven / piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material.

[0010] Furthermore, the concentration of the ammonium persulfate solution in step (1) is 1.5 to 2.5 mol / L.

[0011] Furthermore, the co-solvent in step (2) is a binary co-solvent formed by DMSO and water.

[0012] Furthermore, the volume fraction of DMSO in step (2) is 40-80%.

[0013] Furthermore, the mass concentration of the PVA solution in step (2) is 1 to 10%.

[0014] Furthermore, the crosslinking agent component in step (2) is N,N'-methylenebisacrylamide (BIS) with a mass fraction of 1-3%wt, and the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173) with a volume fraction of 0.35-0.65%.

[0015] Furthermore, the mold in step (3) is composed of two glass slides sandwiching a silicone gasket with a hollowed-out middle portion.

[0016] Furthermore, in step (4), the distance between the UV lamp and the mold is 12 to 18 cm, the wavelength of the UV lamp is 350 to 380 nm, the power is 250 W, the UV lamp irradiation cross-linking time is 6 to 8 minutes, and the ice water bath temperature is maintained at 0 to 4°C.

[0017] Furthermore, the temperature of the aniline polymerization process in step (5) is maintained at 0-4°C.

[0018] The present invention also provides a light-driven integrated piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material prepared by the above method.

[0019] The present invention has the following advantages:

[0020] 1. The PNIPAM hydrogel prepared by the co-solvent effect has ultrafast water transport characteristics and greatly enhanced mechanical properties. The maximum stress reaches 24.93kPa, the Young's modulus is 13.05kPa, and it can shrink to 39% of its original volume in about 35s in hot water at 60°C.

[0021] 2. Low-temperature freeze-thaw inhibits the excessive polymerization of aniline, allowing aniline to form a uniform polyaniline conductive network along the hydrogel network structure, providing the composite hydrogel with excellent sensing performance with high sensitivity, stability, repeatability, etc.

[0022] 3. Due to the efficient photothermal effect of polyaniline and the high responsiveness of the open-pore structure, the (PVA)PNIPAM / PANI composite hydrogel exhibits omnidirectional light-driven capabilities, bending to more than 90° within 4 seconds under ultraviolet light irradiation, and the recovery time is shortened to less than 10 seconds.

[0023] 4. When the hydrogel bends under photothermal drive, the piezoresistive sensing layer can provide real-time feedback on the resistance changes at different bending angles and bending rates, thereby realizing the dual functions of remote control driving and self-sensing of the hydrogel system. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The SEM images of (PVA)PNIPAM composite hydrogels under different solvent ratios;

[0025] Figure 2 Mechanical properties of (PVA)2PNIPAM hydrogel and (PVA)2PNIPAMx hydrogel: (a) stress-strain curve; (b) maximum tensile stress-strain; (c) Young's modulus.

[0026] Figure 3 Mechanical properties of PNIPAM0.6 hydrogel and (PVA)YPNIPAM0.6 hydrogel: (a) stress-strain curve; (b) maximum tensile stress-strain; (c) Young's modulus.

[0027] Figure 4 for (PVA)2PNIPAM 0.6 Hydrogel and (PVA)2PNIPAM 0.6 / PANI z Mechanical properties of hydrogels: (a) stress-strain curve; (b) maximum tensile stress-strain; (c) Young's modulus.

[0028] Figure 5 for (PVA)2PNIPAM 0.6 Hydrogel and (PVA)1PNIPAM 0.6 / PANI z Area change of hydrogel in 60℃ hot water.

[0029] Figure 6 2PNIPAM in air (PVA) 0.6 / PANI 0.2 Hydrogel loading was increased under near-infrared light irradiation.

[0030] Figure 7 (PVA)2PNIPAM under near-infrared light irradiation 0.6 / PANI 0.2 The hydrogel bends at different angles in water.

[0031] Figure 8 (PVA)2PNIPAM under near-infrared light irradiation 0.6 / PANI 0.2 Optical image of the entire process of hydrogel bending in water.

[0032] Fig. 9 (a) Relative resistance variation during stepwise loading-unloading; (b) Repeatability of the hydrogel sensor.

[0033] Fig.10 (a) The resistance curve of the hydrogel sensor changes with the bending angle; (b) The hydrogel sensor is gradually loaded and unloaded as the finger bends; (c) The repeatability of the sensor at different bending angles.

[0034] Fig.11 (a) Bending deformation of hydrogel in water under near-infrared light; (b) bending angle and real-time self-sensing resistance change.

[0035] Fig.12 The actual bending process and the sensor simulation process: (a) Schematic diagram of the actual bending process; (b) piezoresistive output during the bending process.

[0036] Fig.13 To assemble the hydrogel into the octopus arm and grasp objects: (a) Schematic diagram of the actual grasping process; (b) piezoresistive output during the grasping process. DETAILED DESCRIPTION

[0037] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0038] Example 1

[0039] Preparation of (PVA)PNIPAM composite hydrogel based on co-solvent effect:

[0040] (1) N-isopropylacrylamide (NIPAM) was recrystallized three times in a mixed solvent of acetone / n-hexane in a volume ratio of 1:1 to obtain a white needle-shaped purified NIPAM monomer, which was then stored in a refrigerator at 4°C for later use. 2 g of polyvinyl alcohol (PVA) was added to 90 mL of deionized water, heated and stirred in a 95°C water bath for 5 h until completely dissolved, to obtain a clear and transparent 2% PVA solution for later use.

[0041] (2) preparing a hydrogel precursor solution: adding a certain amount of N,N'-methylenebisacrylamide (BIS), N-isopropylacrylamide (NIPAM), and 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173) to a certain ratio of dimethyl sulfoxide (DMSO) / deionized water mixed solvent and stirring to obtain a clear and transparent solution, then adding a certain amount of 10% PVA solution and stirring to obtain a clear and transparent hydrogel precursor solution. The stirring is carried out in the dark during the whole process. The specific ratio is shown in Table 1;

[0042] (3) Injection molding: The mold is composed of two glass slides sandwiching a hollowed-out silicone gasket. Carefully inject the hydrogel precursor solution into the mold to avoid generating bubbles during the injection process.

[0043] (4) Cross-linking: The mold after injection molding was placed in an ice water bath 15 cm below a UV lamp (λ = 365 nm, 250 W) for 5 min. After curing and demolding, it was repeatedly rinsed with deionized water to remove the residual solution on the surface of the hydrogel to obtain a (PVA) PNIPAM composite hydrogel.

[0044] Table 1 Component ratios of (PVA)PNIPAM composite hydrogels with different solvent ratios

[0045]

[0046] We use dimethyl sulfoxide (DMSO)-water binary solvent to replace the single water solvent in the traditional hydrogel preparation process. For PNIPAM, DMSO is a stronger solvent than water. Therefore, during the polymerization process, DMSO will compete for adsorption sites along the polymer backbone, causing the PNIPAM phase to change from an extended linear chain to a collapsed spherical chain, and chemical cross-linking will fix this structure and preserve it permanently. We change the hydrogel structure through the co-solvent effect and enhance the hydrogel's driving performance and mechanical properties.

[0047] In addition, by carefully selecting the solvent composition, the pore structure can be further adjusted to improve the driving performance and mechanical properties of the hydrogel actuator. Since a single PNIPAM network is relatively fragile and prone to irreversible damage under stress loading, this will seriously limit the practical application of PNIPAM hydrogels in soft actuators. Therefore, polyvinyl alcohol (PVA) is added to the reaction system as a strength-enhancing component to further improve the mechanical properties of PNIPAM hydrogels.

[0048] In order to investigate the effect of the proportion of DMSO in the solvent on the microstructure of the prepared PNIPAM hydrogel, we prepared PNIPAM hydrogels with DMSO volume accounting for 0%, 40%, 50%, 60%, 70%, 80%, and 100% of the total solvent volume fraction and defined them as (PVA)PNIPAM. x (x is 0.4, 0.5, 0.6, 0.7, 0.8, and 1, respectively), and the hydrogel without PVA is defined as PNIPAM x By continuously increasing the concentration of DMSO in the solvent, this open pore structure slowly changes back to a closed pore structure, such as Figure 1 When DMSO accounts for too high a proportion in the solvent and becomes dominant, the competition between DMSO and water is broken, the co-solvent effect is weakened, and the PNIPAM molecular chain is transformed from a sphere to a coil again.

[0049] In order to further study the effect of DMSO-water mixed solvent on the mechanical properties of PNIPAM hydrogels, the PVA content was controlled at 2%. Under the same experimental conditions, (PVA)2PNIPAM hydrogels prepared with pure water solvent and (PVA)2PNIPAM hydrogels prepared with mixed solvent were tested. x The hydrogel was subjected to stress-strain tests. Figure 2 As shown, PNIPAM has a high water content and poor mechanical properties. The maximum stress of the (PVA)2PNIPAM hydrogel prepared with pure water solvent is 6.21 kPa, and the maximum strain is 82%. The addition of DMSO causes PNIPAM to form a phase separation structure during the polymerization process, which will make the prepared hydrogel stronger. As the proportion of DMSO in the solvent increases, the stress gradually increases. The maximum stress of (PVA)2PNIPAM0.6 reaches 24.93 kPa, which is 4 times that of the (PVA)2PNIPAM hydrogel prepared with pure water solvent under the same conditions. Calculated Young's modulus of (PVA)2PNIPAM hydrogel is 6.89 kPa, while that of (PVA)2PNIPAM0.6 is 13.05 kPa, which is 1.9 times that of the former ( Figure 2.(c)). When DMSO is further increased, the maximum stress of (PVA)2PNIPAM0.8 decreases to 13.14 kPa and the Young's modulus decreases to 6 kPa. This is because DMSO occupies a dominant position in the solvent at this time, and the competition between DMSO and water is weakened, which greatly weakens the phase separation of PNIPAM during the polymerization process, and the open pore structure of the hydrogel slowly begins to recover to a closed pore structure.

[0050] Example 2

[0051] (PVA) x PNIPAM y Preparation of composite hydrogel:

[0052] (1) N-isopropylacrylamide (NIPAM) was recrystallized three times in a mixed solvent of acetone / n-hexane in a volume ratio of 1:1 to obtain a white needle-shaped purified NIPAM monomer, which was then stored in a refrigerator at 4°C for later use. 1 g, 2 g, and 3 g of polyvinyl alcohol (PVA) were added to 90 mL of deionized water, respectively, and heated and stirred in a 95°C water bath for 5 h until completely dissolved, to obtain clear and transparent 1%, 2%, and 3% PVA solutions for later use.

[0053] (2) preparing a hydrogel precursor solution: adding a certain amount of N,N'-methylenebisacrylamide (BIS), N-isopropylacrylamide (NIPAM), and 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173) to a dimethyl sulfoxide (DMSO) / deionized water mixed solvent (the DMSO volume fraction is 60%) and stirring to obtain a clear and transparent solution. Then, adding a certain amount of PVA solution and stirring to obtain a clear and transparent hydrogel precursor solution. The stirring is carried out in the dark during the whole process. The specific ratio is shown in Table 2.

[0054] (3) Injection molding: The mold is composed of two glass slides sandwiching a hollowed-out silicone gasket. Carefully inject the hydrogel precursor solution into the mold to avoid generating bubbles during the injection process.

[0055] (4) Cross-linking: The mold after injection molding was placed in an ice water bath 15 cm below a UV lamp (λ = 365 nm, 250 W) for 5 min. After curing and demolding, it was repeatedly rinsed with deionized water to remove the residual solution on the surface of the hydrogel to obtain a (PVA) PNIPAM composite hydrogel.

[0056] Table 2 Composition ratio of (PVA)PNIPAM composite hydrogels with different PVA contents

[0057]

[0058] Since the abundant hydroxyl groups in PVA can produce stronger hydrogen bonds with the amide groups of PNIPAM, the introduction of PVA can improve the mechanical properties of (PVA)PNIPAM hydrogels. 0.6 The hydrogel is defined as (PVA) y PNIPAM 0.6 (y=1, 2, 3 correspond to PVA concentration of 1%, 2%, 3%). y PNIPAM 0.6 The mechanical properties of the hydrogel were tested. Figure 3 As shown, the maximum stress of the PNIPAM hydrogel prepared by the mixed solvent is 18.18 kPa, the maximum strain is 249.17%, and the Young's modulus is 8.17 kPa. By adding PVA, the Young's modulus of the (PVA)PNIPAM hydrogel first decreases and then increases, and both are greater than that of the pure PNIPAM hydrogel. Although the Young's modulus of the (PVA)2PNIPAM hydrogel is reduced, the maximum stress and maximum strain are both improved, which indicates that the toughness of the hydrogel is increased and can withstand greater stress and deformation, and the lower Young's modulus is beneficial to driving. The subsequent Young's modulus of the hydrogel with a high PVA content is greatly improved, which may be because the formation of PVA crystals significantly increases the strength of the hydrogel, resulting in an increase in the maximum stress and a significant reduction in strain.

[0059] Example 3

[0060] Mechanical properties and driving performance testing of light-driven / piezoresistive sensing (PVA) PNIPAM / PANI hydrogel materials.

[0061] (1) Preparation steps of (PVA) PNIPAM / PANI composite hydrogel material with high-efficiency light-driven integrated piezoresistive sensing:

[0062] a) Prepare ammonium persulfate solution (APS) for use: add 4.564 g of ammonium persulfate into a certain amount of deionized water and stir until completely dissolved, then continue to add deionized water to make the solution volume to 10 mL, to prepare an ammonium persulfate solution with a concentration of 2 mol / L, and then place it in the upper layer of a refrigerator (4°C) for precooling for use.

[0063] b) Preparation of hydrogel precursor solution: 20 mg, 40 mg, 60 mg, 80 mg N,N'-methylenebisacrylamide (BIS), 1 g N-isopropylacrylamide (NIPAM), 25 μL 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173) were added to 3 mL of dimethyl sulfoxide (DMSO) / deionized water mixed solvent and stirred evenly to obtain a clear and transparent solution. Subsequently, 138 μL ANI, 0.42 mL HCl (37%), and 1 mL PVA (10%) were added in an ice water bath. After all components were completely dissolved, 0.5 mL of pre-cooled APS solution was added and stirred rapidly for 1 min.

[0064] c) Injection molding: Inject the prepared hydrogel precursor solution into a mold, which is composed of two glass slides (60 mm × 25 mm) sandwiching a silicone gasket with a hollow area of ​​40 mm × 10 mm in the middle and a thickness of 1.5 mm; Carefully inject the hydrogel precursor solution into the above mold to avoid generating bubbles during the injection process;

[0065] d) Cross-linking: The mold after injection molding was placed in an ice water bath 15 cm below a UV lamp (λ=365 nm, 250 W) for 6 min. After curing, the mold was demolded to obtain the (PVA)PNIPAM composite hydrogel.

[0066] e) Polymerization: The mold was then placed at 4°C to polymerize aniline, and after waiting for 72 hours, it was taken out and demolded, and repeatedly rinsed with deionized water to obtain a light-driven / piezoresistive sensing (PVA) PNIPAM / PANI hydrogel actuator.

[0067] (2) Hydrogel mechanical properties test: After the introduction of PANI, we further studied the effect of different cross-linking densities on the mechanical properties of (PVA)PNIPAM / PANI composite hydrogels prepared based on the co-solvent effect. The PVA content was kept at 2%, the DMSO volume was 60%, and then the BIS dosage was changed and it was defined as (PVA)2PNIPAM 0.6 / PANI z (where z = 0.2, 0.4, 0.6, 0.8 correspond to 20 mg, 40 mg, 60 mg, 80 mg). 0.6 / PANI z Composite hydrogels were subjected to tensile stress-strain tests and tested with (PVA)2PNIPAM 0.6 Contrast. Figure 4 As shown, (PVA)2PNIPAM 0.6 / PANI 0.2 The maximum tensile stress is 20.53 kPa, the relative strain is 220%, and the Young's modulus is 16 kPa, compared with (PVA)2PNIPAM0.6 It can be found that the mechanical strength of the hydrogel is enhanced after the introduction of PANI. This may be due to the formation of a uniform polyaniline network structure by in-situ polymerization, and the double network structure improves the mechanical strength of the hydrogel. For composite hydrogels with different BIS contents, they have adjustable strength and toughness. In order to test the (PVA)2PNIPAM 0.6 / PANI z To investigate the actuation ability of the composite hydrogel, we analyzed the area change rate of the hydrogel in 60°C hot water. Figure 5 As shown, after the introduction of PANI, the hydrogel can achieve an area shrinkage of 42% within 30 s.

[0068] (3) Hydrogel actuation performance test: In order to characterize the actuation performance of the polyaniline composite hydrogel, (PVA)2PNIPAM0.6 and (PVA)2PNIPAM0.6 / PANI0.2 hydrogels (15 mm × 15 mm × 2 mm) were irradiated with near-infrared light (808 nm). When an object weighing 100 times the weight of the dry polymer was hung on the hydrogel strip, the hydrogel strip was still able to effectively contract and lift the object, such as Figure 6 shown. Figure 7 Figure 8 The complete light-driven process of the composite hydrogel was demonstrated. When the light source was turned on, the hydrogel quickly bent to more than 90° within 4 seconds. When the light source output was maintained, the hydrogel's bending remained in the direction of the light source. When the light source was turned off, the hydrogel quickly recovered to its original undeformed structure within 10 seconds.

[0069] Example 4

[0070] Piezoresistive sensing performance test of light-driven / piezoresistive sensing (PVA) PNIPAM / PANI hydrogel materials.

[0071] (1) Preparation steps of (PVA) PNIPAM / PANI composite hydrogel material with high-efficiency light-driven integrated piezoresistive sensing:

[0072] a) Prepare ammonium persulfate solution (APS) for use: add 4.564 g of ammonium persulfate into a certain amount of deionized water and stir until completely dissolved, then continue to add deionized water to make the solution volume to 10 mL, to prepare an ammonium persulfate solution with a concentration of 2 mol / L, and then place it in the upper layer of a refrigerator (4°C) for precooling for use.

[0073] b) Preparation of hydrogel precursor solution: 20 mg N,N'-methylenebisacrylamide (BIS), 1 g N-isopropylacrylamide (NIPAM), and 25 μL 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173) were added to 3 mL of dimethyl sulfoxide (DMSO) / deionized water mixed solvent and stirred evenly to obtain a clear and transparent solution. Subsequently, 138 μL ANI, 0.42 mL HCl (37%), and 1 mL PVA (10%) were added in an ice water bath. After all components were completely dissolved, 0.5 mL of pre-cooled APS solution was added and stirred rapidly for 1 min.

[0074] c) Injection molding: Inject the prepared hydrogel precursor solution into a mold, which is composed of two glass slides (60 mm × 25 mm) sandwiching a silicone gasket with a hollow area of ​​40 mm × 10 mm in the middle and a thickness of 1.5 mm; Carefully inject the hydrogel precursor solution into the above mold to avoid generating bubbles during the injection process;

[0075] d) Cross-linking: The mold after injection molding was placed in an ice water bath 15 cm below a UV lamp (λ=365 nm, 250 W) for 6 min. After curing, the mold was demolded to obtain the (PVA)PNIPAM composite hydrogel.

[0076] e) Polymerization: The mold was then placed at 4°C to polymerize aniline, and after waiting for 72 hours, it was taken out and demolded, and repeatedly rinsed with deionized water to obtain a light-driven / piezoresistive sensing (PVA) PNIPAM / PANI hydrogel actuator.

[0077] (2) Tensile strain detection of sensors

[0078] We stretched the hydrogel sensor to strains of 20%, 40%, 60%, 80%, and 100% and maintained them for a certain period of time, and then recovered and maintained them at the same strain. Fig. 9 As shown in (a), when the hydrogel is stretched to a certain strain, the relative resistance (ΔR / R0) changes accordingly with the increase of strain; when the strain remains unchanged, ΔR / R0 maintains a constant value; when the strain gradually recovers, ΔR / R0 begins to decrease; these phenomena indicate that the hydrogel sensor has good electrical stability under tensile strain.

[0079] In order to test the repeatability of the hydrogel sensor, the hydrogel was subjected to a loading-unloading cyclic tensile test by programming a mechanical testing machine. We subjected the hydrogel sensor to repeated tests at 20%, 40%, and 60% tensile strains. The relative resistance change of the hydrogel sensor is shown in the figure. Fig. 9 As shown in (b), the hydrogel sensor still maintains a stable output signal during 10 repeated loading-unloading cyclic stretching under different strains, which indicates its good repeatability.

[0080] (3) Sensor bending detection

[0081] We attached the hydrogel sensor to the finger and then controlled the finger to bend to different angles, so that the hydrogel sensor can be bent from 0 to 90 degrees. Fig.10 As shown in (a), the resistance of the hydrogel increases during bending. When the bending angle is less than 60°, the sensitivity factor of the sensor is GF = 0.414, and when the bending angle is between 60 and 90°, GF = 0.833. Since the two ends of the hydrogel are fixed on the finger, the hydrogel is continuously stretched as the finger bends during the bending process, which leads to the destruction of the conductive network and increases the resistance. Fig.10 (b) shows the response to discontinuous finger bending and releasing actions. When the finger is gradually bent to 30°, 60°, and 90°, ΔR / R0 increases continuously. When the bending is released, a symmetrical signal of gradually decreasing resistance can be observed. This is because as the bending is restored, the conductive network inside the hydrogel is restored. Further, we conducted multiple repeated bending experiments at 30°, 60°, and 90°, as shown in Figure 2. Fig.10 As shown in (c), the hydrogel sensor exhibits good repeatability in bending detection.

[0082] In general, by introducing PANI, the (PVA)PNIPAM / PANI composite hydrogel has piezoresistive sensing capability and can identify various movements through real-time electrical signal feedback. Therefore, a self-sensing real-time monitoring experiment was further conducted on its underwater light-driven process. The results are shown in Figure 2. Fig.11 As shown, one end of the hydrogel is fixed underwater and the other end is suspended in water. When the near-infrared light is turned on, the hydrogel bends rapidly underwater ( Fig.11 (a)). At the same time, it can be observed that the resistance changes symmetrically in real time with the bending of the hydrogel ( Fig.11 (b)).

[0083] Example 5

[0084] Application of (PVA)PNIPAM / PANI composite hydrogel with efficient light-driven integrated piezoresistive sensing

[0085] During the bending strain detection process, the piezoresistive sensing mode is used. Fig.12 (a) shows the complex bending strain process of the sample. Fig.12 (b) Shows the change of piezoresistive signal during complex bending.

[0086] To further demonstrate the real-time signal feedback during autonomous driving, we assembled the hydrogel on the octopus model arm as a soft proprioceptive arm to imitate the movement process of the octopus grabbing objects in the water. The octopus arm starts from a straight non-moving state, begins to bend under near-infrared light, and wraps around the cylinder. After a period of time, the light is turned off, and the octopus arm lets go of the cylinder and returns to its original state. During this process, we collected its resistance signal in real time. When the near-infrared light irradiates the octopus arm, the hydrogel begins to bend, and the relative resistance decreases; when the resistance tends to be stable, it indicates that the octopus arm has grasped the object; when the light is turned off, the resistance increases, and the surface octopus arm lets go of the object and begins to recover. After a period of time, the resistance begins to stabilize, and the bending of the surface hydrogel is basically restored. Fig.13 It is the real-time piezoresistive signal of the optical drive grabbing process.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a light-driven integrated piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material, comprising the following steps: (1) preparing an ammonium persulfate solution (APS solution): adding ammonium persulfate to deionized water and stirring until completely dissolved, then adding deionized water to prepare the solution into an ammonium persulfate solution, and then precooling for use; (2) preparing a hydrogel precursor solution: adding a crosslinker, N-isopropylacrylamide (NIPAM), and a photoinitiator to a co-solvent and stirring the mixture to obtain a clear and transparent solution; then sequentially adding ANI, HCl solution, and PVA solution in an ice water bath; after all components are completely dissolved, adding a pre-cooled APS solution and stirring the mixture to obtain a hydrogel precursor solution; (3) Injection molding: Inject the prepared hydrogel precursor solution into the mold, and avoid generating bubbles during the injection process; (4) Cross-linking: The mold after injection molding is placed in an ice water bath under ultraviolet light for light curing to obtain (PVA) / PNIPAM composite hydrogel; (5) Polymerization: The mold is then placed at low temperature to polymerize aniline. After the reaction is completed, the mold is removed and repeatedly rinsed with deionized water to obtain a light-driven / piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material.

2. The method for preparing a light-driven integrated piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material according to claim 1, characterized in that: The concentration of the ammonium persulfate solution in step (1) is 1.5 to 2.5 mol / L.

3. The method for preparing a light-driven integrated piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material according to claim 1, characterized in that: The co-solvent in step (2) is a binary co-solvent formed by DMSO and water.

4. The method for preparing a light-driven integrated piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material according to claim 3, characterized in that: The volume fraction of DMSO in step (2) is 40-80%.

5. The method for preparing a light-driven integrated piezoresistive sensing (PVA) PNIPAM / PANI composite hydrogel material according to claim 1, characterized in that: The mass concentration of the PVA solution in step (2) is 1 to 10%.

6. The method for preparing a (PVA) PNIPAM / PANI composite hydrogel material for light-driven integrated piezoresistive sensing according to claim 1, characterized in that: The crosslinking agent component of step (2) is N,N'-methylenebisacrylamide (BIS) with a mass fraction of 1-3%wt, and the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173) with a volume fraction of 0.35-0.65%.

7. The method for preparing a (PVA) PNIPAM / PANI composite hydrogel material for light-driven integrated piezoresistive sensing according to claim 1, characterized in that: The mold in step (3) is composed of two glass slides sandwiching a silicone gasket with a hollow middle portion.

8. The method for preparing a (PVA) PNIPAM / PANI composite hydrogel material for light-driven integrated piezoresistive sensing according to claim 1, characterized in that: In the step (4), the distance between the UV lamp and the mold is 12 to 18 cm, the wavelength of the UV lamp is 350 to 380 nm, the power is 250 W, the UV lamp irradiation cross-linking time is 6 to 8 minutes, and the ice water bath temperature is maintained at 0 to 4°C.

9. According to the method for preparing a light-driven integrated piezoresistive sensor (PVA) PNIPAM / PANI composite hydrogel material as described in claim 1, the temperature of the aniline polymerization process in step (5) is maintained at 0-4°C.