Preparation method of vegetable waste-based degradable mulching film
By preparing degradable plastic film with materials such as vegetable waste and sodium alginate, agar, etc., the problem of difficult degradation of vegetable waste treatment and traditional plastic film is solved, and the dual goals of efficient resource utilization and environmental protection are achieved.
Patent Information
- Application Number
- CN202411331529.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
The existing technology cannot effectively deal with vegetable waste, resulting in waste of resources and environmental pollution, and traditional plastic plastic films are difficult to degrade, affecting the soil and the environment.
Degradable plastic films are prepared by using vegetable waste and materials such as sodium alginate, agar, glutaraldehyde and glycerol. The mechanical strength and water barrier properties of the plastic film are improved through cross-linking and plasticization.
It realizes the high-value utilization of vegetable waste, reduces environmental pollution, reduces production costs, improves the environmental sustainability and performance of plastic film, and is suitable for large-scale production.
Smart Images

Figure CN119060381A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste resource utilization, and in particular to a method for preparing a vegetable waste-based degradable mulch film. Background Art
[0002] According to the China Statistical Yearbook 2023, from 2010 to 2022, my country's vegetable planting area increased from 17,431,000 hectares to 22,434,000 hectares, a growth rate of 28.7%. During the same period, the proportion of vegetable planting in the total crop planting area also increased from 10.99% to 13.20%. The amount of waste generated every day during the production, transportation, storage, distribution and consumption of vegetables is huge. During the production and processing stages, the waste rate of vegetables can reach 33.6% and 20.5% respectively. The waste rate during transportation and storage is about 31%. Vegetable waste usually has high water content and is easily biodegradable. If these wastes are not properly handled, it will lead to resource waste and environmental pollution, such as greenhouse gas emissions, soil and water pollution, etc.
[0003] At present, the main methods for treating vegetable waste include composting, feed processing, landfilling and incineration. The composting process may produce leachate, which may cause environmental pollution, and the loss of nitrogen may easily lead to problems such as poor compost quality and low fertilizer efficiency; feed processing is carried out in a sterile environment and requires high production costs; landfilling will produce leachate, which may lead to soil and groundwater pollution; incineration will increase the net emission of carbon dioxide in the atmosphere and produce harmful gases.
[0004] Mulch films have been widely used in the agricultural industry to reduce soil moisture loss, increase soil temperature, increase early crop yields and reduce nitrogen loss. Currently, low-density polyethylene is the most commonly used mulch film material. However, polyethylene is difficult to degrade, and its residues will increase soil impermeability, change soil microbial communities, interfere with crop root development and nutrient uptake, and cause damage to crop yield and quality. Biodegradable mulch films are made from biomass and are proposed as an alternative to traditional plastic mulch films.
[0005] Vegetable waste, as a widely existing biomass resource, has not yet been used to prepare biodegradable mulch. In order to improve the resource utilization efficiency of vegetable waste and realize its high-value utilization, the present invention proposes a method for preparing a vegetable waste-based degradable mulch. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a vegetable waste-based degradable mulch film, so as to solve the problem that the existing vegetable waste cannot be treated and disposed of efficiently and environmentally friendly.
[0007] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing a vegetable waste-based degradable mulch film, comprising the following steps:
[0008] S1, crushing, squeezing and filtering the vegetable waste to obtain vegetable waste residue, mixing and grinding the obtained residue with water to obtain a uniform and fine vegetable waste slurry;
[0009] S2, mixing the vegetable waste slurry obtained in S1 with the sodium alginate solution, and obtaining a sodium alginate-vegetable slurry gel after the reaction is completed;
[0010] S3, sequentially adding a crosslinking agent, a plasticizer and agar to the sodium alginate-vegetable pulp gel obtained in S2, and obtaining a liquid mulch film after the reaction is completed;
[0011] S4, drying the liquid mulch film obtained in S3 to obtain the vegetable waste-based degradable mulch film of the present invention.
[0012] Furthermore, in the S1, the mass ratio of vegetable waste residue to water is 1:1, the water is preferably deionized water, and the particle size of the vegetable waste particles in the vegetable waste slurry after grinding is not greater than 1 mm.
[0013] Furthermore, in the S2, the concentration of the sodium alginate solution is 10 g / L.
[0014] Furthermore, the mass ratio of the sodium alginate solution to the vegetable waste slurry is 0.5-4:1.
[0015] Furthermore, in the S2, the reaction temperature is 70-90° C., the reaction time is 5-20 min, and the stirring intensity is 300-500 rpm.
[0016] Furthermore, in the S3, the crosslinking agent is a glutaraldehyde solution with a mass fraction of 25%, and the added amount is 1-3% of the mass of the sodium alginate-vegetable pulp gel; after the glutaraldehyde solution is added, the reaction is continued for 3-10 minutes, the reaction temperature is 70-90°C, and the stirring intensity is 300-500rpm.
[0017] Furthermore, in the S3, the plasticizer is glycerol, and the added amount is 0-4% of the mass of the sodium alginate-vegetable pulp gel; after the addition of glycerol, the reaction is continued for 3-10 minutes, the reaction temperature is 70-90° C., and the stirring intensity is 300-500 rpm.
[0018] Furthermore, in the S3, the amount of agar added is 0-1% of the mass of the sodium alginate-vegetable pulp gel; after the agar is added, the reaction is continued for 2 hours, the reaction temperature is 70-90° C., and the stirring intensity is 300-500 rpm.
[0019] Furthermore, in the above S4, before the liquid mulch film is dried, the liquid mulch film is unfolded, and the thickness of the liquid mulch film after unfolding is 0.1-0.2 g / cm 2 .
[0020] Furthermore, the drying temperature is 50-80° C., and the drying time is 8-14 hours.
[0021] Beneficial effects of the present invention:
[0022] 1. Reduce environmental pollution: Vegetable waste usually has the characteristics of high water content and easy to rot and deteriorate. Untreated vegetable waste will cause serious pollution to the environment. The present invention reduces the pollution of waste to the environment by converting vegetable waste into degradable mulch film;
[0023] 2. High-value utilization of resources: The present invention converts vegetable waste into valuable degradable mulch film, realizes high-value utilization of waste, improves resource utilization efficiency, and conforms to the concept of resource recycling;
[0024] 3. Reduce production costs: Compared with the traditional biodegradable mulch film production method, the present invention uses cheap and readily available vegetable waste as the main raw material, which significantly reduces the production cost;
[0025] 4. Improve environmental sustainability: The degradable mulch produced by the present invention can be naturally degraded during use and after disposal, avoiding the environmental problems caused by the difficulty in degrading traditional polyethylene mulch, and improving the environmental sustainability of the mulch;
[0026] 5. Improved material properties: The degradable mulch prepared by the present invention combines sodium alginate and agar, and has good mechanical strength and flexibility. At the same time, the stability and practicality of the mulch are improved through the cross-linking effect of glutaraldehyde and the plasticizing effect of glycerol. The tensile strength of the vegetable waste-based degradable mulch film of the present invention can reach 14.86MPa; the minimum water vapor permeability can reach 0.5283×10 -6 g·m -1 ·Pa -1 ·h -1 ;
[0027] 6. Process simplification: The preparation method of the present invention has a simple process and is easy to operate. It does not require complicated equipment and process conditions and is suitable for large-scale production, further reducing production costs and process complexity. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is the FT-IR spectra of the vegetable pulp VP of Example 1 of the present invention, the LMF of Comparative Example 1 and the VMF of Example 4;
[0029] Figure 2is the total XPS spectra of the vegetable pulp VP of Example 1, the LMF of Comparative Example 1 and the VMF of Example 4 of the present invention;
[0030] Figure 3 are high-resolution XPS spectra of the vegetable pulp VP of Example 1, LMF of Comparative Example 1, and VMF of Example 4 of the present invention, wherein (a), (b), and (c) are high-resolution XPS spectra of C1s of VP, LMF, and VMF, respectively, and (d), (e), and (f) are high-resolution XPS spectra of O1s of VP, LMF, and VMF, respectively;
[0031] Figure 4 It is a diagram of the formation mechanism of the VMF cross-linked network structure of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0033] The invention uses vegetable waste residue as the main raw material, combines sodium alginate and agar, and uses glutaraldehyde and glycerol as a cross-linking agent and a plasticizer respectively to prepare a ground film with good mechanical properties, water barrier properties and heat preservation properties.
[0034] In the method of the present invention, vegetable pulp provides rich organic matter and cellulose, sodium alginate and agar provide good film-forming property and mechanical strength, the cross-linking effect of glutaraldehyde enhances the stability of the ground film, the aldehyde groups in glutaraldehyde react with the hydroxyl groups in the main chains of cellulose and sodium alginate to form a stable acetal bond network structure; the vegetable waste and the active ingredients in the sodium alginate are cross-linked through internal / external hydrogen bonds and van der Waals forces; the plasticizing effect of glycerol improves the flexibility of the ground film, and glycerol, as a plasticizer, is distributed in the entire network and participates in the formation of a hydrogen bond network inside the material, thereby enhancing the flexibility and ductility of the material; agar provides additional structural support for the ground film to form a more stable continuous film layer; the combined effect of these components enables the ground film to exhibit good mechanical properties and suitable water vapor permeability.
[0035] The method of the present invention not only effectively solves the problem of vegetable waste treatment, but also produces a mulch film product with excellent performance, environmental protection and degradability, thus achieving the dual goals of environmental protection and efficient utilization of resources.
[0036] Example 1
[0037] The vegetable waste is crushed and then squeezed and filtered to obtain vegetable waste residues, the vegetable waste residues are mixed with deionized water of equal mass, and then ground to obtain uniform and fine vegetable pulp, the average particle size of the vegetable waste particles in the vegetable pulp is 0.86mm, the vegetable pulp is sealed and stored for standby use and sampled, and the composition (according to the detection standard) and element content (element analyzer) are detected, and the parameters are as follows:
[0038] Table 1 Content of each component of vegetable pulp (except for water content, the rest of the components are the percentage of raw material dry basis)
[0039]
[0040] Table 2 Proportion of each element in vegetable waste
[0041]
[0042] A sodium alginate solution with a concentration of 10 g / L and uniform and fine vegetable pulp (mixed before use) were taken in a mass ratio of 4:1, and stirred at 80°C and 400 rpm for 10 minutes to obtain a sodium alginate-vegetable pulp gel.
[0043] At 80°C and a rotation speed of 400 rpm, a glutaraldehyde solution with a mass ratio of 3% based on sodium alginate-vegetable pulp gel is added as a cross-linking agent; 5 minutes after the addition of the glutaraldehyde solution, 1% propylene glycol with a mass ratio of 1% based on sodium alginate-vegetable pulp gel is added; 5 minutes after the addition of propylene glycol, 0.5% agar with a mass ratio of 0.5% based on sodium alginate-vegetable pulp gel is added; after adding agar, the reaction is continued at 80°C and a rotation speed of 400 rpm for 2 hours to obtain a liquid mulch film.
[0044] 25 g of liquid mulch was poured into a culture dish with a diameter of 15 cm and dried at 65° C. for 12 h to obtain a biodegradable vegetable waste mulch.
[0045] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 8.73 MPa, an elongation at break of 7.77%, and a water vapor permeability of 0.6056×10 -6 g·m -1 ·Pa -1 ·h -1 .
[0046] Example 2
[0047] In this embodiment, the mass ratio of the sodium alginate solution to the uniform fine vegetable pulp is 1.5:1, and the rest is the same as in Embodiment 1.
[0048] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 10.36 MPa, an elongation at break of 7.74%, and a water vapor permeability of 0.6440×10-6 g·m -1 ·Pa -1 ·h -1 .
[0049] Example 3
[0050] In this embodiment, the mass ratio of the sodium alginate solution to the uniform fine vegetable pulp is 1:1.5, and the rest is the same as in Embodiment 1.
[0051] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 14.86 MPa, an elongation at break of 6.21%, and a water vapor permeability of 0.7971×10 -6 g·m -1 ·Pa -1 ·h -1 .
[0052] It can be seen from Examples 1-3 that with the increase in the amount of vegetable pulp used, the tensile strength and water vapor permeability of the vegetable waste-based degradable mulch film will be significantly improved, but the corresponding elongation at break will decrease. Taking all factors into consideration, when the mass ratio of sodium alginate solution to uniform fine vegetable pulp is 1.5:1, good tensile strength can be guaranteed, while also having a good elongation at break and good water vapor permeability.
[0053] Example 4
[0054] In this embodiment, the amount of glutaraldehyde solution added is 2% of the mass of the sodium alginate-vegetable pulp gel, and the rest is the same as in Embodiment 2.
[0055] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 10.48 MPa, an elongation at break of 8.02%, and a water vapor permeability of 0.5712×10 -6 g·m -1 ·Pa -1 ·h -1 .
[0056] Example 5
[0057] In this embodiment, the amount of glutaraldehyde solution added is 1% of the mass of the sodium alginate-vegetable pulp gel, and the rest is the same as in Embodiment 2.
[0058] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 8.06 MPa, an elongation at break of 6.77%, and a water vapor permeability of 0.6713×10 -6 g·m -1 ·Pa -1 ·h -1 .
[0059] It can be seen from Examples 1, 4-5 that as the amount of cross-linking agent glutaraldehyde solution is reduced, the tensile strength first increases slightly and then decreases sharply. Similarly, the elongation at break in Example 5 also decreases significantly. In addition, the increased water vapor permeability affects the moisture retention of the mulch film. Taking all factors into consideration, the amount of cross-linking agent glutaraldehyde solution is preferably 2%.
[0060] Example 6
[0061] In this example, glycerol was not added, and the other parts were the same as those in Example 4.
[0062] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 7.62 MPa, an elongation at break of 3.77%, and a water vapor permeability of 0.5283×10 -6 g·m -1 ·Pa -1 ·h -1 .
[0063] Example 7
[0064] In this embodiment, the amount of glycerol added is 2% of the mass of the sodium alginate-vegetable pulp gel, and the rest is the same as in Embodiment 4.
[0065] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 8.83 MPa, an elongation at break of 7.44%, and a water vapor permeability of 0.7643×10 -6 g·m -1 ·Pa -1 ·h -1 .
[0066] In the subsequent tests of this embodiment, the amount of glycerol was further increased, and it was found that with the increase in the amount of glycerol added, the tensile strength of the film under the same treatment continued to decrease. This is due to the hydrophilicity of glycerol, and the water vapor permeability is also due to the increasing hydrophilicity.
[0067] It can be seen from Examples 4, 6-7 that when the addition amount of propylene glycol is 0%, although a mulch film is produced, the elongation at break is significantly low. When the amount of propylene glycol is increased, the tensile strength is significantly reduced and the water vapor permeability is also increased. Taking all factors into consideration, the addition amount of propylene glycol is still preferably 1%.
[0068] Example 8
[0069] In this embodiment, agar is not added, and the rest is the same as in Example 4.
[0070] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 8.68 MPa, an elongation at break of 9.11%, and a water vapor permeability of 0.8645×10 -6 g·m-1 ·Pa -1 ·h -1 .
[0071] Example 9
[0072] In this embodiment, the amount of agar added is 1% of the mass of the sodium alginate-vegetable pulp gel, and the rest is the same as in Embodiment 4.
[0073] The vegetable waste-based biodegradable mulch film obtained in this example has a tensile strength of 13.35 MPa, an elongation at break of 4.82%, and a water vapor permeability of 0.6972×10 -6 g·m -1 ·Pa -1 ·h -1 .
[0074] It can be seen from Examples 4, 8-9 that when agar is not added, the tensile strength of the mulch film is significantly low and the water vapor permeability is high, while when excessive agar is added, the elongation at break is seriously affected. Taking all factors into consideration, the addition amount of agar is still preferably 0.5%.
[0075] The above embodiments explore the optimal conditions for implementing the technical solutions of the present invention, but it is undeniable that the technical solutions of the present invention can be implemented within the conditions defined by the present invention.
[0076] Comparative Example 1
[0077] In this comparative example 1, no vegetable pulp was added, and other conditions were the same as those in Example 4, so as to obtain a degradable mulch film without adding vegetable pulp.
[0078] Infrared spectroscopy (FT-IR) was performed on the vegetable pulp (VP), the degradable mulch film (LMF) without vegetable pulp added obtained in this comparative example, and the vegetable waste-based degradable mulch film (VMF) obtained by the method of the present invention to verify the interaction between the components of the vegetable waste-based degradable mulch film and the changes in functional groups. The results are as follows: Figure 1 As shown:
[0079] The spectrum of VP shows typical absorption bands of cellulose, hemicellulose, lignin, protein and lipid, with the band at 2929.06 cm -1 The absorption band at 1628.70 cm is attributed to the asymmetric stretching vibration of CH, indicating the presence of alkyl chains; -1 and 1736.38cm -1 The absorption bands of 1419.78cm correspond to the C=O stretching vibration of protein and the carbonyl structure of hemicellulose; -1 and 1244.90cm -1The absorption bands at 1455.17 cm are generated by the symmetrical CO stretching vibration of lignin and the COC stretching vibration of hemicellulose; -1 、1149.39cm -1 and 1419.78cm -1 The absorption bands at the positions correspond to the -CH2 bending vibration, COO - Symmetric stretching vibration of starch and cellulose 1-4 glycosidic bond stretching vibration; 1081cm -1 and 1023cm -1 The band at is associated with the CO stretching vibrations in the COH and COC groups of cellulose and hemicellulose.
[0080] All characteristic absorption bands of VP are retained in the VMF spectrum, and the OH stretching vibration band (3415.28 cm in VP) -1 ) to the lower wave number 3386.78cm -1 The movement of the VMF components indicated the formation of new intermolecular / intramolecular hydrogen bonds between them.
[0081] Compared with LMF, VMF is 1621.46cm -1 The absorption peak at 3386.73 cm was enhanced, which was attributed to the cross-linking reaction between the carboxyl groups in SAS (sodium alginate solution) and the newly added protein amino groups, which enhanced the absorption intensity of C=O stretching vibration. VMF showed a more significant OH stretching vibration band (3386.73 cm) than LMF. -1 ), indicating the strengthening of hydrogen bonding in VMF. The COC group of VMF is at 1039.10 cm -1 The enhanced band intensity at is the result of the acetal reaction between the hydroxyl and aldehyde groups.
[0082] XPS (X-ray electron spectroscopy) was used to study the chemical composition and bond state of the VP, LMF and VMF surfaces. Figure 2 As shown:
[0083] The spectra revealed that C, O and N were the main elements in VP, LMF and VMF, and a small amount of Na was also detected in the VMF sample.
[0084] Compared with VP, VMF exhibits a higher carbon content and a lower oxygen content (as shown in Table 3). This change is likely to be derived from the cross-linking reaction between the -OH groups in VP and SAS and the -CHO groups in glutaraldehyde. In the preparation process of VMF, cellulose and SAS in VP are polysaccharides, and their molecules contain abundant -OH. Glutaraldehyde is used as a cross-linking agent, and its aldehyde group undergoes acetalization reaction with the hydroxyl groups in SAS and cellulose (see equation 1), forming a stable and dense cross-linked network, which increases the carbon content in VMF. Not only does it increase the relative content of carbon atoms, but it also replaces some of the original CH bonds by forming new chemical bonds (such as CC and CN), thereby reducing the oxygen content in the material. In addition, the cross-linking reaction leads to an increase in the relative proportion of carbon elements, which further reduces the relative proportion of oxygen.
[0085] R-CHO+2R′-OH→R-CH(OR′)2+H2O(1)
[0086] Table 3 Relative concentrations of different elements on VP, LMF and VMF surfaces
[0087]
[0088] Figure 3 The XPS high-resolution spectra of carbon-containing (C1s) and oxygen-containing (O1s) functional groups in VP, LMF and VMF samples and their relative content analysis are shown. Figure 3 As shown in (ac), the C1s peak at 284.8 eV corresponds to the CC / CH structure, indicating the presence of an alkyl chain; while the appearance of CO / CN in the range of 285.5-286.5 eV reflects the characteristics of alcohol, amine or amide groups. The peak position of 286.5-289.5 eV shows the characteristic absorption peaks of acetal, ester and carboxylic acid groups. Figure 3 As shown in (df), the sub-peaks of the O1s peak at 532.86 eV and 532.41 eV reveal the OCO / OCN structures in amides, esters and carboxylic acids, and the COC and C-OH structures in acetals and alcohols, respectively. Compared with VP, the relative contents of CC / CH, CO and OCO in VMF acetals increased significantly, and the C-OH content in alcohols decreased accordingly, confirming the cross-linking reaction between VP and the hydroxyl groups in SAS (sodium alginate solution) and the aldehyde groups in glutaraldehyde.
[0089] The formation mechanism of VMF cross-linked network structure:
[0090] VMF prepared under optimal conditions can be evenly sprayed on the soil surface by a pneumatic spray gun. After the water evaporates, a uniform brown film layer with a three-dimensional network structure with chemical cross-linking and physical entanglement is formed. This process involves two key steps:
[0091] (1) Chemical crosslinking: FT-IR analysis shows that at 1039.10 cm -1 The vibration peaks observed at indicate the presence of acetal bonds (see Figure 1 ). XPS analysis results show that the relative contents of CC / CH, CO and OCO in VMF acetals increase, and the C-OH content in alcohol molecules decreases (see Figure 3 ), which further confirmed the cross-linking reaction between VP and the hydroxyl groups in SAS and the aldehyde groups in glutaraldehyde.
[0092] (2) Physical entanglement: After adding SAS, the OH stretching vibration band in VMF changes from 3415.28 cm -1 Move to 3386.78cm -1 , and a more significant OH stretching vibration band (3386.73 cm -1 ), indicating the enhancement and redistribution of hydrogen bonding in VMF. Hydrogen bonding within VMF mainly occurs between various active ingredients, such as hydroxyl groups in cellulose, hemicellulose and sodium alginate molecular chains, amino groups in proteins and hydroxyl groups in glycerol molecular chains. These groups act as acceptors and donors to each other in the formation of hydrogen bonds, and together they form a stable hydrogen bonding network.
[0093] like Figure 4 As shown in Figure 1, the complex network structure in VMF is mainly formed by cross-linking reaction between the aldehyde groups in glutaraldehyde and the hydroxyl groups in the main chain of cellulose and sodium alginate to form stable acetal bonds (see Formula 1). The active ingredients in VP and SAS are cross-linked through internal / external hydrogen bonds and van der Waals forces. Glycerol, as a plasticizer, is distributed throughout the network and participates in the formation of a hydrogen bond network inside the material, thereby enhancing the flexibility and ductility of the material. The added agar provides additional structural support for the mulch film, forming a more stable continuous film layer. The combined effect of these components enables VMF to exhibit good mechanical properties and suitable water vapor permeability.
[0094] The present invention is not limited to the above-mentioned optimal implementation mode. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that are the same or similar to those of the present application fall within the protection scope of the present invention.
Claims
1. A method for preparing a vegetable waste-based degradable mulch film, characterized in that: The following steps are involved: S1, crushing, squeezing and filtering the vegetable waste to obtain vegetable waste residue, mixing and grinding the obtained residue with water to obtain a uniform and fine vegetable waste slurry; S2, mixing the vegetable waste slurry obtained in S1 with the sodium alginate solution, and obtaining a sodium alginate-vegetable slurry gel after the reaction is completed; S3, sequentially adding a crosslinking agent, a plasticizer and agar to the sodium alginate-vegetable pulp gel obtained in S2, and obtaining a liquid mulch film after the reaction is completed; S4, drying the liquid mulch film obtained in S3 to obtain the vegetable waste-based degradable mulch film of the present invention.
2. The method for preparing a vegetable waste-based degradable mulch film according to claim 1, characterized in that: In the S1, the mass ratio of vegetable waste residue to water is 1:1, the water is preferably deionized water, and the particle size of the vegetable waste particles in the vegetable waste slurry after grinding is not greater than 1 mm.
3. The method for preparing a vegetable waste-based degradable mulch film according to claim 2, characterized in that: In the S2, the concentration of the sodium alginate solution is 10 g / L.
4. The method for preparing a vegetable waste-based degradable mulch film according to claim 3, characterized in that: The mass ratio of the sodium alginate solution to the vegetable waste slurry is 0.5-4:
1.
5. The method for preparing a vegetable waste-based degradable mulch film according to claim 1, characterized in that: In the S2, the reaction temperature is 70-90°C, the reaction time is 5-20 min, and the stirring intensity is 300-500 rpm.
6. The method for preparing a vegetable waste-based degradable mulch film according to claim 1, characterized in that: In the S3, the crosslinking agent is a glutaraldehyde solution with a mass fraction of 25%, and the added amount is 1-3% of the mass of the sodium alginate-vegetable pulp gel; after the glutaraldehyde solution is added, the reaction is continued for 3-10 minutes, the reaction temperature is 70-90° C., and the stirring intensity is 300-500 rpm.
7. The method for preparing a vegetable waste-based degradable mulch film according to claim 1, characterized in that: In the S3, the plasticizer is glycerol, and the added amount is 0-4% of the mass of the sodium alginate-vegetable pulp gel; after the glycerol is added, the reaction is continued for 3-10 minutes, the reaction temperature is 70-90° C., and the stirring intensity is 300-500 rpm.
8. The method for preparing a vegetable waste-based degradable mulch film according to claim 1, characterized in that: In the S3, the amount of agar added is 0-1% of the mass of the sodium alginate-vegetable pulp gel; after the agar is added, the reaction is continued for 2 hours, the reaction temperature is 70-90° C., and the stirring intensity is 300-500 rpm.
9. The method for preparing a vegetable waste-based degradable mulch film according to claim 1, characterized in that: In the above S4, before the liquid ground film is dried, the liquid ground film is unfolded, and the thickness of the liquid ground film after unfolding is 0.1-0.2 g / cm 2 .
10. The method for preparing a vegetable waste-based degradable mulch film according to claim 9, characterized in that: The drying temperature is 50-80°C, and the drying time is 8-14h.