Graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane as well as preparation method and application thereof
Through the preparation of graphene oxide modified sulfonated polyvinyl alcohol and Nafion composite membrane, the degradation problem of proton exchange membrane under free radical oxidation and mechanical damage is solved, the high mechanical strength and proton conductivity are improved, and the craftsmanship improves environmental friendliness.
Patent Information
- Application Number
- CN202411220521.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
AI Technical Summary
The existing proton exchange membranes are susceptible to radical oxidation and mechanical damage in actual operation, resulting in degradation, cracks and perforation, and the preparation process is complex and unfriendly to the environment, making it difficult to achieve high durability and high proton conductivity.
The preparation method of graphene oxide modified sulfonated polyvinyl alcohol/Nafion composite film is adopted. By adding a sulfonating agent and a Nafion solution to the polyvinyl alcohol solution, and drying and cross-linking in the graphene oxide dispersion, the formation of Composite membrane with self-healing function.
It achieves self-healing after mechanical damage, and significantly improves proton conductivity and tensile strength, solves the problems of membrane durability and mechanical stability, while simplifying the preparation process and reducing the impact on the environment.
Smart Images

Figure CN119060388A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of proton exchange membranes and relates to a graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane and a preparation method and application thereof. Background Art
[0002] As one of the most important core components of the electrolyzer, the proton exchange membrane (PEM) has the dual functions of transporting protons and separating gases, accounting for about 20% of the total membrane electrode cost. At present, the commercial PEM mainly uses perfluorosulfonic acid (PFSA) proton exchange membrane, among which Nafion membrane has the advantages of excellent ion conductivity, high proton conductivity and good mechanical properties, and is currently the most widely used proton exchange membrane for hydrogen production by electrolysis of water. Although the homogeneous Nafion membrane has many advantages, a large number of free radicals (such as hydrogen free radicals, oxygen free radicals, etc.) will be generated during the actual operation of PEM water electrolysis. Some functional groups on its chain will be oxidized by these free radicals, resulting in membrane degradation, and eventually cracks and perforations in the membrane. In addition, the uneven pressure between the membrane electrode assembly and the bipolar plate will also cause cracks or perforations in the membrane, so that the gases on both sides of the membrane will cross and react on the catalyst surface. The heat generated will cause the membrane to soften or even melt, aggravating the damage of the membrane and leading to safety hazards. In addition, gas crossover will also reduce the electrolysis efficiency and thermodynamic efficiency. Therefore, it is particularly important to design and prepare a proton exchange membrane with high durability, high mechanical stability and strong proton conductivity. CN114349365A prepared a durable 3,4-dihydroxyphenylalanine chelated cerium ion composite proton exchange membrane, by adding an organic antioxidant and an inorganic free radical scavenger chelate (3,4-dihydroxyphenylalanine complex) to the PFSA ionomer to synergistically enhance the antioxidant effect, but this method will reduce the proton conductivity of the membrane to a certain extent, and, with the operation of the battery, the chelate will continue to be lost and eventually fail.
[0003] CN114221003A etches the MXene precursor with a mixture of a strong acid solution and a fluoride salt, grows CeO2 single particles on its surface, and finally mixes the CeO2 / MXene composite material with Nafion resin to obtain a proton exchange membrane. Although this method effectively improves the proton conductivity and stability of the composite membrane, it uses strong acids and fluorine-containing compounds, which can easily cause environmental pollution.
[0004] CN106633555A proposes a method for preparing a polyvinyl alcohol film with self-repairing function by constructing dynamic covalent bonds using Diels-Alder reaction. First, polyvinyl alcohol is grafted with a furan derivative to obtain polyvinyl alcohol modified with a furan ring, and then a cross-linking agent that reacts with the furan group to undergo Diels-Alder reaction is added, and a polyvinyl alcohol film modified with self-repairing function is obtained after Diels-Alder reaction. Although the composite film prepared by this method has a certain repair effect, it is less environmentally friendly, and the proton conductivity of the composite film needs to be improved.
[0005] The polymer chain of polyvinyl alcohol (PVA) contains a large number of hydroxyl groups, which can serve as a proton transfer bridge. In addition, PVA has a relatively low production cost, good biodegradability, and most importantly, excellent film-forming properties and good structural flexibility. The hydroxyl groups of PVA can form abundant hydrogen bonds with the sulfonic acid groups in Nafion. The dynamic and reversible hydrogen bond network can not only make the composite membrane have higher mechanical properties, but also spontaneously repair the tens of micron micropores generated during the operation of the battery, so that the membrane can restore its original mechanical properties and proton conductivity.
[0006] In view of the problems of high cost, poor mechanical damage resistance, low mechanical strength, complex preparation process and environmental unfriendliness of current proton exchange membranes, the present invention provides a method for preparing a composite membrane with self-healing function and excellent mechanical strength. Summary of the invention
[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane and a preparation method and application thereof.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In one aspect, the present invention provides a method for preparing a graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane, the preparation method comprising the following steps:
[0010] 1) dissolving polyvinyl alcohol (PVA) in water to obtain a polyvinyl alcohol solution;
[0011] 2) adding a sulfonating agent to the polyvinyl alcohol solution obtained in step 1), stirring and mixing to obtain a uniform solution (hereinafter referred to as SPVA solution);
[0012] 3) Adding Nafion solution to the solution obtained in step 2) and stirring evenly to obtain a mixed solution (i.e., a mixed solution of SPVA and Nafion);
[0013] 4) adding the graphene oxide dispersion to the mixed solution obtained in step 3), and stirring to obtain a precursor solution;
[0014] 5) Casting the precursor solution obtained in step 4) on a substrate, drying, and then cross-linking and sulfonating, cooling, to obtain the self-healing graphene oxide modified polyvinyl alcohol / Nafion composite proton exchange membrane.
[0015] The proton exchange membrane prepared by the present invention is aimed at the cracks gradually generated by the degradation of the Nafion membrane due to free radical attack during the electrolysis process, as well as the cracks generated in the membrane during the PEM electrolytic cell assembly or due to excessive local pressure. The blended alcohol polymer is added to form a cross-linked network structure with Nafion. The polymer chain of the blended alcohol polymer contains a large number of hydroxyl groups, which can form abundant hydrogen bonds with the sulfonic acid groups in Nafion. When there are sufficient hydrogen bonds in the composite membrane, it can usually have both self-healing properties and mechanical strength.
[0016] The self-healing graphene oxide modified polyvinyl alcohol / Nafion composite proton exchange membrane prepared by the present invention can self-heal under a certain humidity after being mechanically damaged, and the tensile properties can be maintained at a high level before and after being subjected to puncture holes.
[0017] Preferably, in step 1), the mass ratio of water to polyvinyl alcohol is 8-9:1, for example 8:1, 8.3:1, 8.5:1, 8.7:1, 8.9:1 or 9:1.
[0018] Preferably, the dissolution in step 1) is completed under heating and stirring, and the heating is heating to 60-90°C, for example, 60°C, 65°C, 68°C, 70°C, 75°C, 78°C, 80°C, 85°C, 88°C or 90°C, and the stirring time is 4-8h, for example, 4h, 5h, 6h, 7h or 8h.
[0019] Preferably, the sulfonating agent in step 2) is any one of lignin sulfonic acid, sulfoacetic acid, sulfosuccinic acid, and 4-sulfophthalic acid.
[0020] Preferably, in step 2), the mass ratio of the sulfonating agent to polyvinyl alcohol is 1:5-1:20, for example, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 or 1:20, etc.
[0021] Preferably, the stirring and mixing in step 2) is carried out at room temperature.
[0022] Preferably, the stirring and mixing time in step 2) is 24-48 h, for example, 24 h, 26 h, 28 h, 30 h, 33 h, 36 h, 38 h, 40 h, 42 h, 44 h, 46 h or 48 h.
[0023] Preferably, the mass percentage concentration of the Nafion solution in step 3) is 5-20wt%, for example, 5wt%, 7wt%, 9wt%, 10wt%, 12wt%, 14wt%, 15wt%, 17wt%, 19wt% or 20wt%.
[0024] Preferably, in step 3), the mass ratio of Nafion to PVA is 6:4.
[0025] Preferably, the Nafion solution in step 3) is a Nafion D2020 solution.
[0026] Preferably, the stirring time in step 3) is 12-24 h, for example, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h.
[0027] Preferably, the graphene oxide dispersion in step 4) is obtained by dispersing graphene oxide in deionized water.
[0028] Preferably, the concentration of graphene oxide in the graphene oxide dispersion in step 4) is 2-10 mg / mL, for example 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 9 mg / mL or 10 mg / mL.
[0029] Preferably, in step 4), the mass ratio of graphene oxide to polyvinyl alcohol is 0.01-0.02:1, for example, 0.01:1, 0.013:1, 0.015:1, 0.018:1 or 0.02:1.
[0030] Preferably, the stirring time in step 4) is 12-24 h, for example, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h.
[0031] Preferably, in step 5), the substrate is a glass plate.
[0032] Preferably, the drying in step 5) is evaporating at room temperature for 8-12 h (e.g., 8 h, 9 h, 10 h, 11 h or 12 h), and then continuing to dry in an oven at 60-80 ° C (e.g., 60 ° C, 65 ° C, 68 ° C, 70 ° C, 75 ° C, 78 ° C or 80 ° C) for 8-12 h (e.g., 8 h, 9 h, 10 h, 11 h or 12 h).
[0033] Preferably, the temperature of the cross-linking sulfonation in step 5) is 100-120°C, for example, 100°C, 105°C, 108°C, 110°C, 113°C, 115°C, 118°C or 120°C.
[0034] Preferably, the cross-linking sulfonation time in step 5) is 0.5-1 h, such as 0.5 h, 0.7 h, 0.9 h or 1 h.
[0035] Preferably, the cooling in step 5) is cooling to room temperature.
[0036] Preferably, step 5) further comprises the step of peeling the obtained film from the substrate after cooling.
[0037] On the other hand, the present invention provides a graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane prepared by the preparation method described above.
[0038] Preferably, the thickness of the graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane is 50-60 μm.
[0039] On the other hand, the present invention provides the use of the graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane as described above in hydrogen production by water electrolysis.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] The PVA in the present invention benefits from its high affinity for water and inherent film-forming ability, and can effectively improve the mechanical properties of Nafion when mixed with Nafion. In addition, the high density of hydroxyl groups in PVA enables it to utilize the inherent reversibility of dynamic hydrogen bonds to self-repair from mechanical damage.
[0042] In the technical solution of the present invention, in order to solve the problem of lack of conductive groups on the PVA chain and low proton conductivity, proton conductive groups are introduced into the PVA chain, and the modified PVA is compounded with Nafion with high proton conductivity. At the same time, graphene oxide with long-range ordered nano-transmission channels is added, which can increase the proton conductivity to 8-9 orders of magnitude of pure PVA.
[0043] Since PVA has a high water absorption rate and causes large swelling, the tensile strength of the composite membrane is significantly improved after modification with graphene oxide and sulfoacetic acid, and the maximum tensile strength exceeds 40MPa. This is of great significance for the mechanical damage resistance of Nafion proton exchange membrane in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The graphs are the changes in tensile strength of different samples prepared in the embodiments and comparative examples before and after repair;
[0045] Figure 2 The proton conductivity test results of different samples prepared in the embodiments and comparative examples are shown in FIG.
[0046] Figure 3 Optical microscope photos of the composite membrane prepared in Example 6 before and after repair;
[0047] Figure 4 Optical microscope photos of the commercial Nafion212 membrane before and after repair in comparative example 1. DETAILED DESCRIPTION
[0048] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0049] Example 1:
[0050] The preparation of PVA / Nafion composite proton exchange membrane includes the following steps:
[0051] 1) Dissolve 0.4 g of PVA powder in 3.6 g of deionized water, heat and stir at 80° C. for 6 h until the solution is uniform and transparent, to obtain a PVA solution with a mass percentage of 10 wt%;
[0052] 2) Add 3 g of 20 wt% Nafion D2020 solution to the solution prepared in step 1), stir at room temperature for 12 h, and the mass ratio of Nafion to PVA in the mixed solution is 3:2;
[0053] 3) Casting the mixed solution of step 2) on a glass plate, drying at room temperature for 12 hours, and further drying in an oven at 60° C. for 12 hours after molding;
[0054] 4) Finally, the temperature was raised to 110°C and stored for 0.5 h. After cooling to room temperature, the membrane was peeled off from the glass plate to obtain a PVA / Nafion composite membrane.
[0055] The proton conductivity of the membrane is measured by the AC impedance test method of Chenhua 660 workstation. The module is immersed in ultrapure water for 12 hours, and the parameters are set: frequency 0.1-106Hz, and the potential amplitude is 5mV. It is calculated by the formula: σ=a / (R×b×d), where d represents the membrane thickness, a represents the distance between the two electrodes, and b represents the effective length of the membrane in the direction perpendicular to the two electrodes.
[0056] The tensile curve of the film was obtained by dynamic thermomechanical analyzer testing, wherein the tensile speed was 50 mm / min, the test temperature was 25°C, and the sample was cut into strips with a length of 20 mm and a width of 5 mm.
[0057] The proton conductivity of the proton exchange membrane obtained by the test at room temperature is 0.035S / cm, the maximum tensile strength before repair is 28MPa, and the maximum tensile strength after the repair test is 23MPa.
[0058] Example 2:
[0059] The preparation of SPVA / Nafion composite proton exchange membrane includes the following steps:
[0060] 1) Dissolve 0.4 g of PVA powder in 3.6 g of deionized water, heat and stir at 80° C. for 6 h until the solution is uniform and transparent, to obtain a PVA solution with a mass percentage of 10 wt%;
[0061] 2) adding 0.06 g of lignin sulfonic acid to the solution in 1), and continuing to stir at room temperature for 24 h to obtain a uniform SPVA solution;
[0062] 3) adding 3 g of 20 wt% Nafion D2020 solution to the solution prepared in step 2), stirring at room temperature for 12 h, wherein the mass ratio of Nafion to PVA in the mixed solution is 3:2;
[0063] 4) Casting the mixed solution of step 3) on a glass plate, drying at room temperature for 12 hours, and further drying in an oven at 60° C. for 12 hours after molding;
[0064] 5) Finally, the temperature was raised to 110°C and stored for 0.5 h. After cooling to room temperature, the membrane was peeled off from the glass plate to obtain the SPVA / Nafion composite membrane.
[0065] The proton conductivity of the proton exchange membrane obtained by the test at room temperature is 0.04S / cm, the maximum tensile strength before repair is 33MPa, and the maximum tensile strength after the repair test is 27MPa.
[0066] Example 3
[0067] The preparation of SPVA / Nafion composite proton exchange membrane includes the following steps:
[0068] 1) Dissolve 0.4 g of PVA powder in 3.6 g of deionized water, heat and stir at 80° C. for 6 h until the solution is uniform and transparent, to obtain a 10 wt % PVA solution;
[0069] 2) adding 0.086 g of sulfosuccinic acid solution to the solution in 1), and continuing stirring at room temperature for 24 h to obtain a uniform SPVA solution;
[0070] 3) adding 3 g of 20 wt% Nafion D2020 solution to the solution prepared in step 2), stirring at room temperature for 12 h, wherein the mass ratio of Nafion to PVA in the mixed solution is 3:2;
[0071] 4) Casting the mixed solution of step 3) on a glass plate, drying at room temperature for 12 hours, and further drying in an oven at 60° C. for 12 hours after molding;
[0072] 5) Finally, the temperature was raised to 110°C and stored for 0.5 h. After cooling to room temperature, the membrane was peeled off from the glass plate to obtain the SPVA / Nafion composite membrane.
[0073] The proton conductivity of the proton exchange membrane obtained by the test at room temperature is 0.069S / cm, the maximum tensile strength before repair is 29MPa, and the maximum tensile strength after the repair test is 23.5MPa.
[0074] Example 4
[0075] The preparation of SPVA / Nafion composite proton exchange membrane includes the following steps:
[0076] 1) Dissolve 0.4 g of PVA powder in 3.6 g of deionized water, heat and stir at 80° C. for 6 h until the solution is uniform and transparent, to obtain a PVA solution with a mass percentage of 10 wt%;
[0077] 2) adding 0.12 g of 4-sulfophthalic acid solution to the solution in step 1), and continuing stirring at room temperature for 24 h to obtain a uniform SPVA solution;
[0078] 3) Add 3 g of 20 wt% Nafion D2020 solution to the solution prepared in step 2), stir at room temperature for 12 h, and the mass ratio of Nafion to PVA in the mixed solution is 3:2;
[0079] 4) Casting the mixed solution of step 3) on a glass plate, drying at room temperature for 12 hours, and further drying in an oven at 60° C. for 12 hours after forming;
[0080] 5) Finally, the temperature was raised to 110°C and stored for 0.5 h. After cooling to room temperature, the membrane was peeled off from the glass plate to obtain the SPVA / Nafion composite membrane.
[0081] The proton conductivity of the proton exchange membrane obtained by the test at room temperature is 0.065S / cm, the maximum tensile strength before repair is 31MPa, and the maximum tensile strength after the repair test is 25MPa.
[0082] Example 5
[0083] The preparation of SPVA / Nafion composite proton exchange membrane includes the following steps:
[0084] 1) Dissolve 0.4 g of PVA powder in 3.6 g of deionized water, heat and stir at 80° C. for 6 h until the solution is uniform and transparent, to obtain a PVA solution with a mass percentage of 10 wt%;
[0085] 2) adding 0.06 g of sulfoacetic acid to the solution in 1), and continuing stirring at room temperature for 24 h to obtain a uniform SPVA solution;
[0086] 3) adding 3 g of 20 wt% Nafion D2020 solution to the solution prepared in step 2), stirring at room temperature for 12 h, wherein the mass ratio of Nafion to PVA in the mixed solution is 3:2;
[0087] 4) Casting the mixed solution of step 3) on a glass plate, drying at room temperature for 12 hours, and further drying in an oven at 60° C. for 12 hours after molding;
[0088] 5) Finally, the temperature was raised to 110°C and stored for 0.5 h. After cooling to room temperature, the membrane was peeled off from the glass plate to obtain the SPVA / Nafion composite membrane.
[0089] The proton conductivity of the proton exchange membrane obtained by the test at room temperature is 0.075S / cm, the maximum tensile strength before repair is 35MPa, and the maximum tensile strength after the repair test is 28MPa.
[0090] Example 6
[0091] The preparation of SPVA / Nafion composite proton exchange membrane modified by graphene oxide comprises the following steps:
[0092] 1) Dissolve 0.4 g of PVA powder in 3.6 g of deionized water, heat and stir at 80° C. for 6 h until the solution is uniform and transparent, to obtain a PVA solution with a mass percentage of 10 wt%;
[0093] 2) adding 0.06 g of sulfoacetic acid to the solution in step 1), and continuing to stir at room temperature for 24 h to obtain a uniform SPVA solution;
[0094] 3) adding 3 g of 20 wt% Nafion D2020 solution to the solution prepared in step 2), stirring at room temperature for 12 h, wherein the mass ratio of Nafion to PVA in the mixed solution is 3:2;
[0095] 4) Add 20 ml of 2 mg / mL graphene oxide dispersion to the mixed solution of step 3) and stir for 12 h;
[0096] 5) Cast the mixed solution onto a glass plate, dry at room temperature for 12 hours, and continue drying in an oven at 60°C for 12 hours after forming;
[0097] 6) Finally, the temperature was raised to 110° C. and stored for 0.5 h. After cooling to room temperature, the membrane was peeled off from the glass plate to obtain a graphene oxide-modified SPVA / Nafion composite membrane.
[0098] The proton conductivity of the proton exchange membrane obtained by the test at room temperature is 0.086S / cm, the maximum tensile strength before repair is 42MPa, and the maximum tensile strength after the repair test is 36MPa.
[0099] Comparative Example 1
[0100] The comparative example used in this experiment is a commercial Nafion 211 membrane. Under the same conditions, its proton conductivity is tested to be 0.079 S / cm, its maximum tensile strength before repair is 18.8 MPa, and its maximum tensile strength after repair is 13.8 MPa.
[0101] Repair effect test method:
[0102] The maximum tensile strength of the Nafion212 membrane in Example 1, Example 2, Example 3, Example 4, Example 5, Example 6 and the comparative example before and after repair was tested. The repair conditions are: take a membrane with a length * width of 4.5cm * 1.5cm and a thickness of ≈50μm, pierce three holes at the same position with a needle with a diameter of 100 microns, store it under the same conditions (deionized water at 60℃) for 4h, and dry it at 60℃ for 12h. The change in tensile strength before and after the membrane repair was tested, and the change before and after the repair was observed with an optical microscope (Leica DM2700P).
[0103] Figure 1 The tensile strength results of different samples prepared in some examples and comparative example 1 before and after the repair test are shown. It can be seen that the composite film of example 6 has the highest mechanical strength, and the mechanical strength can be best restored after the repair test.
[0104] Figure 2 The graphs show the proton conductivity test results of different samples prepared in some embodiments and comparative example 1. It can be seen that the composite membrane of example 6 has the highest proton conductivity.
[0105] Figure 3 These are optical microscope photos of the composite membrane prepared in Example 4 before and after repair; it can be seen that after being stored in deionized water for 4 hours, the composite membrane prepared in Example 6 can repair the holes well.
[0106] Figure 4The optical microscope photos of the commercial Nafion 212 membrane before and after repair in comparative example 1 show that after being stored in deionized water at 60°C for 4 hours, there is no difference between the Nafion 212 membrane and the original membrane, indicating that the Nafion 212 membrane does not have the ability to repair.
[0107] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane, It is characterized in that The preparation method comprises the following steps: 1) dissolving polyvinyl alcohol in water to obtain a polyvinyl alcohol solution; 2) adding a sulfonating agent to the polyvinyl alcohol solution obtained in step 1), stirring and mixing to obtain a uniform solution; 3) adding Nafion solution to the solution obtained in step 2) and stirring uniformly to obtain a mixed solution; 4) adding the graphene oxide dispersion to the mixed solution obtained in step 3), and stirring to obtain a precursor solution; 5) Casting the precursor solution obtained in step 4) on a substrate, drying, and then cross-linking and sulfonating, cooling, to obtain the self-healing graphene oxide modified sulfonated polyvinyl alcohol / Nafion composite proton exchange membrane.
2. The preparation method according to claim 1, It is characterized in that The mass ratio of water to polyvinyl alcohol in step 1) is 8-9:1; Preferably, the dissolution in step 1) is completed under heating and stirring, the heating is heated to 60-90° C., and the stirring time is 4-8 h.
3. The preparation method according to claim 1 or 2, It is characterized in that Step 2) the sulfonating agent is any one of lignin sulfonic acid, sulfoacetic acid, sulfosuccinic acid, and 4-sulfophthalic acid; Preferably, in step 2), the mass ratio of the sulfonating agent to polyvinyl alcohol is 1:5-1:
20.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that Step 2) the stirring and mixing is carried out at room temperature; Preferably, the stirring and mixing time in step 2) is 24-48 hours.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that Step 3) The mass percentage concentration of the Nafion solution is 5-20wt%; preferably, the mass ratio of the Nafion to PVA is 8:2-1:1; Preferably, the Nafion solution in step 3) is Nafion D2020 solution; Preferably, the stirring time in step 3) is 12-24 hours.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that Step 4) the graphene oxide dispersion is obtained by dispersing graphene oxide in deionized water; Preferably, the concentration of graphene oxide in the graphene oxide dispersion in step 4) is 2-10 mg / mL; Preferably, in step 4), the mass ratio of graphene oxide to polyvinyl alcohol is 0.01-0.02:
1.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The stirring time in step 4) is 12-24 hours.
8. The preparation method according to any one of claims 1 to 6, It is characterized in that Step 5) The substrate is a glass plate; Preferably, the drying in step 5) is performed by evaporating at room temperature for 8-12 hours, and then drying in an oven at 60-80° C. for 8-12 hours; Preferably, the temperature of the cross-linking sulfonation in step 5) is 100-120°C; Preferably, the cross-linking sulfonation time in step 5) is 0.5-1h; Preferably, the cooling in step 5) is cooling to room temperature; Preferably, step 5) further comprises the step of peeling the obtained film from the substrate after cooling.
9. A graphene oxide modified polyvinyl alcohol / Nafion composite proton exchange membrane prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the graphene oxide modified polyvinyl alcohol / Nafion composite proton exchange membrane according to any one of claims 1 to 8 in hydrogen production by water electrolysis.
Citation Information
Patent Citations
Polyvinyl alcohol membrane with self-repair function implemented by aid of dynamic covalent bonds and method for preparing polyvinyl alcohol membrane
CN106633555A
Proton exchange membrane for proton exchange membrane fuel cell and preparation method thereof
CN114221003A
Preparation method of high-durability 3, 4-dihydroxyphenylalanine chelated cerium ion composite proton exchange membrane
CN114349365A