Boron-containing graphene oxide and flexible silicone rubber-boron-containing graphene oxide neutron shielding material and preparation method thereof

By performing gamma ray graft polymerization on graphene oxide and compounding with flexible silicone rubber, the problem of insufficient flexibility and shielding performance of existing neutron radiation protection materials is solved, and efficient, flexible and highly elastic neutron shielding is prepared. Material, suitable for equipment and personnel protection in complex shapes.

CN119060408APending Publication Date: 2024-12-03BEIJING UNIV OF CHEM TECH +1

Patent Information

Application Number
CN202310634861.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing neutron radiation protection materials lack flexibility and high elasticity, making them difficult to be suitable for equipment and personnel protection with complex shapes. The neutron shielding performance of traditional boron polymers is limited, and the adsorption capacity of graphene is limited.

Method used

By grafting and polymerizing graphene oxide with boric acid containing vinyl structure under γ-ray irradiation, boron oxide with a large specific surface area and good dispersion is formed, and composited with flexible silicone rubber, a good one is prepared. Neutron shielding performance, thermal conductivity and high flexibility neutron shielding materials.

Benefits of technology

It realizes efficient neutron shielding performance, avoids the reduction of the mechanical properties and elasticity of the material, provides flexible, elastic and efficient neutron protection effects, and is suitable for protection of protective clothing, blankets and irregular-shaped instrument surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004259776270000081
    Figure BDA0004259776270000081
Patent Text Reader

Abstract

The invention provides boron-containing graphene oxide and a flexible silicon rubber-boron-containing graphene oxide neutron shielding material and a preparation method thereof. The preparation method of the boron-containing graphene oxide comprises the following steps: dispersing graphene oxide in a first solvent to obtain a graphene oxide dispersion liquid; adding boric acid containing a vinyl structure into the graphene oxide dispersion liquid to obtain a mixed solution; and placing the mixed solution in a 60Co radioactive source for irradiation, washing and filtering to obtain a modified graphene oxide aggregate, and drying to obtain the boron-containing graphene oxide. The boron-containing graphene oxide has a large specific surface area, good dispersibility and good compatibility with polymers, and can be compounded with silicone rubber to prepare a flexible neutron shielding material. The flexible silicone rubber-boron-containing graphene oxide neutron shielding material provided by the invention has the advantages of good flexibility, relatively high neutron shielding performance, excellent mechanical performance, high elasticity and simple preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nuclear radiation protection and the technical field of nuclear radiation shielding material preparation, and in particular relates to a boron-containing graphene oxide, a flexible silicone rubber-boron-containing graphene oxide neutron shielding material and a preparation method thereof. Background Art

[0002] With the development of nuclear technology, neutron radiation technology has been widely used in industrial detection, agricultural breeding, medical diagnosis, and neutron radiation weapons. While the application of neutrons creates value for society, it also brings harm to human health. Compared with gamma-ray and x-ray radiation damage, neutron radiation damage has a high casualty rate, severe symptoms, and is more difficult to rescue. Therefore, neutron radiation protection is a vital part of the field of nuclear technology. Most neutron sources are immovable, so the traditional method is to build cement-based neutron shielding bunkers for shielding containment, CT rooms, and particle accelerators. In order to ensure the safety of workers and equipment, additional reliable safeguards should be provided. Cement-based materials are not suitable for the protection of equipment such as neutron detectors and instruments with complex shapes and abnormal structures, which require additional shielding in narrow spaces and around curved surfaces.

[0003] However, some mechanical equipment with complex shapes also need flexible neutron shielding materials for protection. Traditional neutron shielding materials are mainly heavy metals, boron-containing polyethylene and concrete.

[0004] Contains 10 Polymer composites of B, such as boron-containing polyethylene, boron-containing polypropylene, etc., can effectively shield neutron radiation because boron compounds show good thermal neutron absorption capacity. However, boron-containing polyethylene or boron-containing polypropylene do not have the characteristics of flexibility and high elasticity, and cannot be prepared into protective clothing or protective blankets to protect personnel, nor can they be covered on irregularly shaped instrument surfaces to provide secondary protection. In recent years, a series of new flexible polymer matrix neutron materials have been developed, such as flexible shielding materials (CN104910629A) based on silica gel, but the hydrogen content of silica gel is low and the neutron shielding performance is limited. Polymer nanocomposites can improve neutron absorption efficiency because nanofillers with large specific surface area reduce particle absorption due to self-shielding, thereby increasing the possibility of neutron interaction. Graphene has better thermal, electrical and mechanical properties than traditional carbon materials. It is an excellent nanofiller that enhances the electrical conductivity, mechanical properties and thermal properties of composite materials, and has become a research hotspot in the field of materials in the world today. Pyrene boric acid can be conjugated with graphene and adsorbed on the surface of graphene, but due to the limitation of the size structure of graphene sheets, it is difficult to adsorb in large quantities. Therefore, it is difficult to achieve a good neutron shielding effect by compounding with flexible polymer materials. Summary of the invention

[0005] In order to solve the above technical problems, the object of the present invention is to provide a boron-containing graphene oxide and a preparation method thereof, wherein the boron-containing graphene oxide has a large specific surface area, good dispersibility, and good compatibility with polymers.

[0006] The present invention also aims to provide a flexible silicone rubber / boron-containing graphene oxide neutron radiation shielding material and a preparation method thereof, which has the advantages of good neutron shielding performance, good thermal conductivity, high flexibility, high elasticity, simple process and low cost.

[0007] To achieve the above object, the present invention first provides a method for preparing boron-containing graphene oxide, which comprises the following steps:

[0008] Dispersing graphene oxide in a first solvent to obtain a graphene oxide dispersion, wherein the dispersion amount is 0.1 mg of graphene oxide / 1 mL of the first solvent to 10 mg of graphene oxide / 1 mL of the first solvent;

[0009] Adding boric acid containing a vinyl structure to the graphene oxide dispersion to obtain a mixed solution; wherein the concentration of the boric acid containing a vinyl structure is 0.01 to 10 g / mL based on the volume of the graphene oxide dispersion;

[0010] The mixed solution is placed 60 The graphene oxide was irradiated in a Co radiation source, and modified graphene oxide aggregates were obtained after washing and filtering, and boron-containing graphene oxide was obtained after drying.

[0011] In the method for preparing boron-containing graphene oxide, preferably, the mass ratio of the boric acid containing a vinyl structure to the graphene oxide is 100:1 to 1:1, more preferably 80:1 to 1:1, and further preferably 50:1 to 1:1.

[0012] In the method for preparing boron-containing graphene oxide, preferably, the dispersion amount is 0.5 mg graphene oxide / 1 mL first solvent to 5 mg graphene oxide / 1 mL first solvent.

[0013] In the method for preparing boron-containing graphene oxide, preferably, the first solvent is selected from one or a mixture of two or more of water, methanol, ethanol, propanol, butanol, tetrahydrofuran, ethyl acetate, N,N-dimethylformamide, more preferably one or a mixture of two or more of tetrahydrofuran, ethyl acetate, N,N-dimethylformamide.

[0014] In the method for preparing boron-containing graphene oxide, preferably, the concentration of the boric acid containing a vinyl structure is 0.1 to 5 g / mL.

[0015] In the preparation method of boron-containing graphene oxide, preferably, the silane containing a vinyl structure is selected from 2-vinylbenzene boronic acid, 3-vinylbenzene boronic acid, 1-pentenyl boronic acid, trans-β-styrene boronic acid, 1-phenyl vinyl boronic acid, cis-1-propylene-1-boric acid, allenyl boronic acid, E-2-(1-octenyl)-4,4,5,5-tetramethyl-[1,3,2]-dioxaboric acid, trans-1-nonenyl boronic acid, 3-acrylamidophenyl boronic acid, 4-octenyl boronic acid ethanolamine acid Ester, trans-2-butene-2-ylboronic acid, trans-2-[3-(trifluoromethyl)phenyl]vinylboronic acid; more preferably 2-vinylbenzeneboronic acid, 3-vinylbenzeneboronic acid, 3-acrylamidophenylboronic acid, allenylboronic acid, cis-1-propylene-1-boric acid, 1-phenylvinylboronic acid, one or a combination of two or more thereof; further preferably 1-phenylvinylboronic acid, 2-vinylbenzeneboronic acid, 3-vinylbenzeneboronic acid, 3-acrylamidophenylboronic acid, one or a combination of two or more thereof.

[0016] In the method for preparing boron-containing graphene oxide, preferably, the absorbed dose of the irradiation is 0.01 to 1000 kGy, more preferably 0.1 to 500 kGy.

[0017] According to a specific embodiment of the present invention, the method for preparing the boron-containing graphene oxide may include the following specific steps:

[0018] (1) ultrasonically dispersing graphene oxide in a first solvent to obtain a graphene oxide dispersion, wherein the ultrasonication is performed at 0 to 60° C. for 0.1 to 10 hours, preferably at 20 to 40° C. for 0.5 to 5 hours.

[0019] (2) Adding boric acid containing a vinyl structure into the graphene oxide dispersion and stirring the mixture to obtain a mixed solution.

[0020] (3) Place the mixture in 60 The modified graphene oxide aggregates are placed in a vacuum drying oven and dried to a constant weight to obtain boron-containing graphene oxide, which is then sealed and stored. The washing solvent is selected from one or more of water, methanol, ethanol, propanol, butanol, acetone, butanone, tetrahydrofuran, ethyl acetate, dichloromethane, chloroform, ethyl chloride, and dichloroethane.

[0021] The present invention also provides a boron-containing graphene oxide, which is prepared by the preparation method of the boron-containing graphene oxide.

[0022] Under the action of gamma ray irradiation, the present invention grafts and polymerizes a boron-containing compound with a vinyl structure on the surface of graphene oxide. With the increase of the absorbed dose, the grafting density tends to increase first and then stabilize. The graphene oxide grafted with the boron-containing polymer has a large specific surface area, good dispersibility, and good compatibility with the polymer. It can be compounded with silicone rubber to prepare a flexible neutron shielding material.

[0023] The present invention also provides a method for preparing a flexible silicone rubber-boron-containing graphene oxide neutron shielding material, which comprises the following steps:

[0024] Dispersing the boron-containing graphene oxide in a second solvent to obtain a boron-containing graphene oxide dispersion;

[0025] Mixing the boron-containing graphene oxide dispersion with vinyl polysiloxane and a catalyst to obtain component A;

[0026] The boron-containing graphene oxide dispersion is mixed with vinyl polysiloxane and hydrogen-containing silicone oil to obtain component B;

[0027] The component A and the component B are mixed in a volume ratio of 1:1 to obtain the flexible silicone rubber-boron-containing graphene oxide neutron shielding material.

[0028] In the above-mentioned method for preparing neutron shielding material, preferably, the second solvent is selected from one of water, methanol, ethanol, propanol, butanol, acetone, butanone, tetrahydrofuran, ethyl acetate, dichloromethane, chloroform, ethyl chloride, and dichloroethane, or a mixture of two or more thereof.

[0029] In the above-mentioned method for preparing neutron shielding material, preferably, the raw material composition of component A comprises: 100-250 parts by weight of vinyl polysiloxane, 1-5 parts by weight of catalyst, and 1-10 parts by weight of boron-containing graphene oxide.

[0030] In the above method for preparing the neutron shielding material, preferably, the catalyst is a platinum-containing salt or acid compound.

[0031] In the above-mentioned method for preparing the neutron shielding material, preferably, the raw material composition of the B component includes: 100-250 parts by weight of vinyl polysiloxane, 20-80 parts by weight of hydrogen-containing silicone oil, and 1-10 parts by weight of boron-containing graphene oxide;

[0032] In the above method for preparing the neutron shielding material, preferably, the viscosity of the vinyl polysiloxane is 1000-100000 mPa / s.

[0033] According to a specific embodiment of the present invention, preferably, the method for preparing the flexible silicone rubber / boron-containing graphene oxide neutron radiation shielding material comprises the following specific steps:

[0034] (a) dispersing the prepared boron-containing graphene oxide in a second solvent to prepare a dispersion.

[0035] (b) mixing the boron-containing graphene oxide dispersion prepared in (a) with vinyl polysiloxane and a catalyst to obtain component A; mixing the boron-containing graphene oxide dispersion prepared in (a) with vinyl polysiloxane and hydrogen-containing silicone oil to obtain component B.

[0036] (c) Add the vinyl polysiloxane, catalyst and boron-containing graphene oxide in component A into a reaction kettle, stir evenly and set aside.

[0037] (d) Add the vinyl polysiloxane, hydrogen-containing silicone oil and boron-containing graphene oxide in component B into a reaction kettle, stir evenly and set aside.

[0038] (e) The substances prepared in step (c) and step (d) are uniformly mixed in a volume ratio of 1:1, stirred in a vacuum environment, and cured at room temperature to obtain a flexible silicone rubber / boron-containing graphene oxide neutron radiation shielding material.

[0039] The present invention also provides a flexible silicone rubber-boron-containing graphene oxide neutron shielding material, which is prepared by the preparation method of the neutron shielding material.

[0040] The technical solution of the present invention has the following beneficial effects:

[0041] (1) The present invention grafts a boron-containing compound containing a vinyl structure onto the surface of graphene oxide by γ-ray irradiation, which not only increases the dispersibility of graphene oxide, but also increases the content of boron on the surface of graphene oxide, which is beneficial to improving the neutron shielding effect.

[0042] (2) The flexible silicon rubber / boron-containing graphene oxide neutron shielding material of the present invention avoids the reduction of mechanical properties, elasticity and flexibility of the material caused by adding fillers such as boron carbide by adding boron-containing graphene oxide with neutron shielding function. The seed shielding material has the advantages of good flexibility, high neutron shielding performance, excellent mechanical properties, high elasticity and simple preparation process, and can be used as neutron shielding protective clothing, protective blanket, or to protect irregularly shaped instrument surfaces or gaps. DETAILED DESCRIPTION

[0043] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0044] Example 1

[0045] This embodiment provides a flexible silicone rubber-boron-containing graphene oxide neutron shielding material, which is prepared by the following steps:

[0046] Graphene oxide is ultrasonically dispersed in N,N-dimethylformamide to obtain a graphene oxide dispersion, wherein the concentration of graphene oxide is 2 mg / mL, the ultrasound is performed at 25° C., and the ultrasound time is 1 hour; 3-acrylamide phenylboronic acid is added to the graphene oxide dispersion and stirred evenly, and the concentration of 3-acrylamide phenylboronic acid is 0.01 g / mL; the mixed solution is placed 60 The modified graphene oxide aggregates were irradiated in a Co radiation source for a certain period of time with an absorbed dose of 20 kGy. After stopping the irradiation, the aggregates were washed with deionized water and filtered, and the process was repeated for several times to obtain the modified graphene oxide aggregates, which were placed in a vacuum drying oven and dried to a constant weight and sealed for storage.

[0047] 200 parts of vinyl polysiloxane, 2 parts of catalyst and 3 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component A for standby; 170 parts of vinyl polysiloxane, 30 parts of hydrogen-containing silicone oil and 5 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component B for standby; the prepared component A and component B are mixed evenly in a volume ratio of 1:1, stirred in vacuum, poured into a mold and cured at room temperature to obtain silicone rubber, i.e., flexible silicone rubber-boron-containing graphene oxide neutron shielding material.

[0048] Example 2

[0049] This embodiment provides a flexible silicone rubber-boron-containing graphene oxide neutron shielding material, which is prepared by the following steps:

[0050] Graphene oxide was ultrasonically dispersed in a mixed solution of methanol and water (V 甲醇 :V 水 =1:1), to obtain a graphene oxide dispersion, wherein the concentration of graphene oxide is 5 mg / mL, ultrasound is performed at 25°C, and the ultrasound time is 1 hour; 3-acrylamide phenylboronic acid is added to the graphene oxide dispersion and stirred evenly, and the concentration of 3-acrylamide phenylboronic acid is 0.1 g / mL; the mixed solution is placed 60 The modified graphene oxide aggregates were irradiated in a Co radiation source for a certain period of time with an absorbed dose of 50 kGy. After stopping the irradiation, the aggregates were washed with deionized water and filtered, and the process was repeated for several times to obtain the modified graphene oxide aggregates, which were placed in a vacuum drying oven and dried to a constant weight and sealed for storage.

[0051] 130 parts of vinyl polysiloxane, 2 parts of catalyst and 3 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component A for standby; 100 parts of vinyl polysiloxane, 30 parts of hydrogen-containing silicone oil and 5 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component B for standby; the prepared component A and component B are mixed evenly in a volume ratio of 1:1, stirred in vacuum, poured into a mold and cured at room temperature to obtain silicone rubber, i.e., flexible silicone rubber-boron-containing graphene oxide neutron shielding material.

[0052] Example 3

[0053] This embodiment provides a flexible silicone rubber-boron-containing graphene oxide neutron shielding material, which is prepared by the following steps:

[0054] Graphene oxide is ultrasonically dispersed in tetrahydrofuran to obtain a graphene oxide dispersion, wherein the concentration of graphene oxide is 0.1 mg / mL, the ultrasound is performed at 25° C., and the ultrasound time is 1 hour; 3-vinylbenzeneboronic acid is added to the graphene oxide dispersion and stirred evenly, wherein the concentration of 3-vinylbenzeneboronic acid is 5 g / mL; the mixed solution is placed 60 The modified graphene oxide aggregates were irradiated in a Co radiation source for a certain period of time with an absorbed dose of 10 kGy. After stopping the irradiation, the aggregates were washed with deionized water and filtered, and the process was repeated for several times to obtain the modified graphene oxide aggregates, which were placed in a vacuum drying oven and dried to a constant weight and sealed for storage.

[0055] 200 parts of vinyl polysiloxane, 2 parts of catalyst and 3 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component A for standby; 170 parts of vinyl polysiloxane, 30 parts of hydrogen-containing silicone oil and 5 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component B for standby; the prepared component A and component B are mixed evenly in a volume ratio of 1:1, stirred in vacuum, poured into a mold and cured at room temperature to obtain silicone rubber, i.e., flexible silicone rubber-boron-containing graphene oxide neutron shielding material.

[0056] Example 4

[0057] This embodiment provides a flexible silicone rubber-boron-containing graphene oxide neutron shielding material, which is prepared by the following steps:

[0058] Graphene oxide is ultrasonically dispersed in tetrahydrofuran to obtain a graphene oxide dispersion, wherein the concentration of graphene oxide is 5 mg / mL, the ultrasound is performed at 25° C., and the ultrasound time is 1 hour; cis-1-propylene-1-boric acid is added to the graphene oxide dispersion and stirred evenly, wherein the concentration of cis-1-propylene-1-boric acid is 5 g / mL; the mixed solution is placed 60The modified graphene oxide aggregates were irradiated in a Co radiation source for a certain period of time with an absorbed dose of 10 kGy. After stopping the irradiation, the aggregates were washed with deionized water and filtered, and the process was repeated for several times to obtain the modified graphene oxide aggregates, which were placed in a vacuum drying oven and dried to a constant weight and sealed for storage.

[0059] 250 parts of vinyl polysiloxane, 2 parts of catalyst and 3 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component A for standby; 220 parts of vinyl polysiloxane, 30 parts of hydrogen-containing silicone oil and 10 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component B for standby; the prepared component A and component B are mixed evenly in a volume ratio of 1:1, stirred in vacuum, poured into a mold and cured at room temperature to obtain silicone rubber, i.e., flexible silicone rubber-boron-containing graphene oxide neutron shielding material.

[0060] Comparative Example 1

[0061] This comparative example provides a neutron shielding material, which is prepared by the following steps:

[0062] Graphene oxide was ultrasonically dispersed in a mixed solution of methanol and water (V 甲醇 :V 水 =1:1) to obtain a graphene oxide dispersion, wherein the concentration of the graphene oxide is 5 mg / mL, and ultrasound is performed at 25° C. for 1 hour; 3-acrylamide phenylboronic acid is added to the graphene oxide dispersion and stirred evenly, wherein the concentration of 3-acrylamide phenylboronic acid is 0.1 g / mL; washing with deionized water, filtering, repeating multiple times, placing in a vacuum drying oven to dry to constant weight, and sealing for storage.

[0063] 130 parts of vinyl polysiloxane, 2 parts of catalyst and 3 parts of graphene oxide are added into a reaction kettle, stirred evenly and used as component A for standby; 100 parts of vinyl polysiloxane, 30 parts of hydrogen-containing silicone oil and 5 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component B for standby; the prepared component A and component B are mixed evenly in a volume ratio of 1:1, stirred in vacuum, poured into a mold and cured at room temperature to obtain silicone rubber, i.e., neutron shielding material.

[0064] Comparative Example 2

[0065] This comparative example provides a neutron shielding material, which is prepared by the following steps:

[0066] Graphene oxide was ultrasonically dispersed in a mixed solution of methanol and water (V 甲醇 :V 水 =1:1) to obtain a graphene oxide dispersion, wherein the concentration of graphene oxide is 5 mg / mL, and ultrasound is performed at 25° C. for 1 hour; washing with deionized water, filtering, repeating multiple times, placing in a vacuum drying oven to dry to constant weight, and sealing for storage.

[0067] 130 parts of vinyl polysiloxane, 2 parts of catalyst and 3 parts of graphene oxide are added into a reaction kettle, stirred evenly and used as component A for standby; 100 parts of vinyl polysiloxane, 30 parts of hydrogen-containing silicone oil and 5 parts of boron-containing graphene oxide are added into a reaction kettle, stirred evenly and used as component B for standby; the prepared component A and component B are mixed evenly in a volume ratio of 1:1, stirred in vacuum, poured into a mold and cured at room temperature to obtain silicone rubber, i.e., neutron shielding material.

[0068] The main performance indicators and experimental methods of the neutron shielding materials prepared in Examples 1-4 of the present invention and Comparative Examples 1-2 are shown in Table 1.

[0069] Table 1 Neutron shielding material performance test results

[0070]

[0071] According to the experimental results in Table 1, it can be seen that the flexible silicone rubber-boron-containing graphene oxide neutron shielding materials prepared in Examples 1-4 have the advantages of good flexibility, high neutron shielding performance, excellent mechanical properties, high elasticity, and simple preparation process.

[0072] The same and similar parts between the various embodiments in this specification can be referenced to each other.

[0073] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing boron-containing graphene oxide, comprising the following steps: Dispersing graphene oxide in a first solvent to obtain a graphene oxide dispersion, wherein the dispersion amount is 0.1 mg of graphene oxide / 1 mL of the first solvent to 10 mg of graphene oxide / 1 mL of the first solvent; Adding boric acid containing a vinyl structure to the graphene oxide dispersion to obtain a mixed solution; wherein the concentration of the boric acid containing a vinyl structure is 0.01 to 10 g / mL based on the volume of the graphene oxide dispersion; preferably, the mass ratio of the boric acid containing a vinyl structure to the graphene oxide is 100:1 to 1:1; The mixed solution is placed 60 The graphene oxide was irradiated in a Co radiation source, and modified graphene oxide aggregates were obtained after washing and filtering, and boron-containing graphene oxide was obtained after drying.

2. The preparation method according to claim 1, wherein The dispersion amount is 0.5 mg graphene oxide / 1 mL first solvent to 5 mg graphene oxide / 1 mL first solvent; Preferably, the first solvent is selected from one or a mixture of two or more of water, methanol, ethanol, propanol, butanol, tetrahydrofuran, ethyl acetate, N,N-dimethylformamide, more preferably one or a mixture of two or more of tetrahydrofuran, ethyl acetate, N,N-dimethylformamide.

3. The preparation method according to claim 1, wherein The concentration of the boric acid containing a vinyl structure is 0.1 to 5 g / mL; Preferably, the silane containing a vinyl structure is selected from 2-vinylbenzene boronic acid, 3-vinylbenzene boronic acid, 1-pentenyl boronic acid, trans-β-styrene boronic acid, 1-phenylvinyl boronic acid, cis-1-propylene-1-boric acid, allenyl boronic acid, E-2-(1-octenyl)-4,4,5,5-tetramethyl-[1,3,2]-dioxaboric acid, trans-1-nonenyl boronic acid, 3-acrylamidophenyl boronic acid, 4-octenyl boronic acid ethanolamine ester, trans-2-butyl boronic acid, Boric acid, 2-vinyl boronic acid, trans-2-[3-(trifluoromethyl)phenyl]vinyl boronic acid; more preferably 2-vinyl boronic acid, 3-vinyl boronic acid, 3-acrylamido boronic acid, allenyl boronic acid, cis-1-propylene-1-boric acid, 1-phenylvinyl boronic acid, or a combination of two or more thereof; further preferably 1-phenylvinyl boronic acid, 2-vinyl boronic acid, 3-vinyl boronic acid, 3-acrylamido boronic acid, or a combination of two or more thereof.

4. The preparation method according to claim 1, wherein The absorbed dose of the irradiation is 0.01 to 1000 kGy, preferably 0.1 to 500 kGy.

5. A boron-containing graphene oxide prepared by the method according to any one of claims 1 to 4.

6. A method for preparing a flexible silicone rubber-boron-containing graphene oxide neutron shielding material, comprising the following steps: dispersing the boron-containing graphene oxide according to claim 5 in a second solvent to obtain a boron-containing graphene oxide dispersion; Mixing the boron-containing graphene oxide dispersion with vinyl polysiloxane and a catalyst to obtain component A; The boron-containing graphene oxide dispersion is mixed with vinyl polysiloxane and hydrogen-containing silicone oil to obtain component B; The component A and the component B are mixed in a volume ratio of 1:1 to obtain the flexible silicone rubber-boron-containing graphene oxide neutron shielding material.

7. The preparation method according to claim 6, wherein: The second solvent is selected from one of water, methanol, ethanol, propanol, butanol, acetone, butanone, tetrahydrofuran, ethyl acetate, dichloromethane, chloroform, ethyl chloride, and dichloroethane, or a mixture of two or more thereof.

8. The preparation method according to claim 6, wherein: The raw material composition of the A component includes: 100-250 parts by weight of vinyl polysiloxane, 1-5 parts by weight of catalyst, and 1-10 parts by weight of boron-containing graphene oxide; Preferably, the viscosity of the vinyl polysiloxane is 1000-100000 mpa / s; Preferably, the catalyst is a platinum-containing salt or acid compound.

9. The preparation method according to claim 6, wherein: The raw material composition of the B component includes: 100-250 parts by weight of vinyl polysiloxane, 20-80 parts by weight of hydrogen-containing silicone oil, and 1-10 parts by weight of boron-containing graphene oxide; Preferably, the viscosity of the vinyl polysiloxane is 1000-100000 mPa / s.

10. A flexible silicone rubber-boron-containing graphene oxide neutron shielding material prepared by the method according to any one of claims 6 to 9.

Citation Information

Patent Citations

  • Flame-retardant flexible lead-free gamma shielding material and preparation method thereof

    CN104910629A

Cited By

  • High-temperature-resistant alloy powder for additive manufacturing and preparation method of high-temperature-resistant alloy powder

    CN119973102A

  • Composite heating film for new energy automobile battery pack and preparation method of composite heating film

    CN120663609A

  • A composite heating film for a new energy automobile battery pack and a preparation method thereof

    CN120663609B