Nano ZnO / delignified kapok cellulose composite material and preparation method thereof
By using high-concentration zinc chloride and sodium hydroxide/urea solution to treat kapok cellulose under low temperature conditions and efficient mixing with colloid mill, the low concentration of reactants and composite strength in the preparation of nano ZnO/cellulose composite materials was solved. The problem of insufficient results has achieved the preparation of high-efficiency and low-energy consumption nano ZnO/delignin kapok cellulose composite materials.
Patent Information
- Application Number
- CN202310634326.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
In the existing nano ZnO/cellulose composite materials preparation methods, the reactant concentration is low, a large amount of water or organic solvent is required, the cellulose carrier does not participate in the control of nano ZnO crystal size and morphology, and the composite amount and composite strength of nano ZnO on cellulose are limited. The problem.
Using kapok fiber as raw material, high-purity cellulose is obtained through delignin, and high-concentration zinc chloride (ZnCl2) solution and sodium hydroxide (NaOH)/urea solution are used as reactants under low temperature conditions, and high-efficiency is carried out by colloid milling. Mix to prepare uniformly sized nano ZnO/delignin kapopter cellulose composites.
The reactant concentration is increased, the operation is simplified, the energy consumption is reduced, and the cellulose solution can be used as a control aid and barrier for nano ZnO, which promotes the in-situ generation and efficient mixing of nano ZnO particles, achieving efficient preparation.
Smart Images

Figure FT_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of natural polymer and nano metal oxide composite materials, and particularly relates to a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof. Background Art
[0002] After nano-processing, ZnO will produce surface and volume effects that do not exist in the macroscopic aggregate state, and will exhibit excellent photocatalytic, UV shielding, antibacterial, photoluminescence and other properties, and will have important application value in the fields of textiles, chemical industry, environmental protection, optoelectronics, biomedicine, etc.
[0003] The preparation of nano ZnO / cellulose composite materials mainly includes preparing nano ZnO by hydrothermal method, and then compounding nano ZnO on cellulose substrate by mixing nano ZnO with cellulose; or immersing cellulose substrate in ZnO precursor solution, and allowing ZnO crystals to nucleate on cellulose substrate to prepare nano ZnO / cellulose composite materials. The shortcomings of the existing methods are that the concentration of reactants is low, a large amount of water or organic solvent is required in the preparation process, the cellulose carrier does not participate in the control of nano ZnO crystal size and morphology, and the composite amount and composite strength of nano ZnO on cellulose are limited. Summary of the invention
[0004] In view of the shortcomings of the existing preparation methods of nano ZnO / cellulose composite materials, the present invention uses kapok fiber as raw material, obtains high-purity cellulose by delignification, and then uses high-concentration zinc chloride (ZnCl2) solution and sodium hydroxide (NaOH) / urea solution as cellulose solvent and nano zinc oxide (ZnO) reactants under low temperature conditions, and uses a colloid mill as a high-efficiency mixing reactor to prepare nano ZnO / delignified kapok cellulose composite materials with uniform size.
[0005] The technical solution adopted by the present invention is: a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, comprising the following steps: (1) A mixed solution of sodium hydroxide and sodium sulfide was prepared, and the mixture was added to kapok fibers and reacted at 100 °C for 2 hours to remove most of the lignin in the kapok fibers; (2) After washing and filtering, the excess water is dried, the kapok fiber is bleached with sodium hypochlorite to remove residual lignin, and then washed and dried; (3) Add the delignified kapok cellulose to a ZnCl2 solution at a certain temperature and stir to obtain a transparent and uniform cellulose solution. At the same time, add another group of delignified kapok cellulose to a NaOH / urea solution at -15°C and stir to obtain another transparent and uniform cellulose solution. (4) uniformly mixing the two cellulose solutions in step (3) in a mechanical dispersion device and reacting them for a certain time within a certain temperature and pH range; (5) The product of step (4) is precipitated, washed, and dried to obtain a nano ZnO / delignified kapok cellulose composite material.
[0006] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (1), the concentration of the ZnCl2 aqueous solution is 50-60 wt%, and the concentration of the NaOH / urea solution is 10 / 15 wt%.
[0007] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (3), the temperature at which the cellulose is dissolved in the ZnCl2 solution is 90-100°C.
[0008] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the mechanical dispersion device is a colloid mill, a homogenizer, etc.
[0009] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (4), the reaction temperature of the two cellulose solutions is 45-60°C.
[0010] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the pH value of the reaction system is 9-13.
[0011] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the reaction time is 40-60 min.
[0012] Compared with the prior art, the preparation method of the nano ZnO / cellulose composite material of the present invention has the following advantages: The method of the present invention has high reactant concentration, simple operation, low energy consumption and is easy for industrial production. The dissolved cellulose molecules contain a large number of hydroxyl groups that can react with zinc ions, so the cellulose solution can be used as a control aid and agglomeration barrier for preparing nano ZnO. The colloid mill can promote the in-situ generation and efficient mixing of nano ZnO particles, so that the preparation method has the characteristics of high concentration, simple operation, low energy consumption and easy industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is the size distribution diagram of ZnO in the composite material prepared in this patent. Implementation
[0014] The present invention is described in detail below with reference to specific embodiments. Example 1
[0015] (1) Prepare a mixed solution of sodium hydroxide and sodium sulfide, add it to kapok fiber and react it at 100 °C for 2 hours to remove most of the lignin in the kapok fiber.
[0016] (2) After washing and filtering, the excess water is dried, the kapok fiber is bleached with sodium hypochlorite to remove residual lignin, and then washed and dried.
[0017] (3) The kapok cellulose from which lignin was removed was added into a ZnCl2 solution at a certain temperature and stirred to obtain a transparent and uniform cellulose solution. At the same time, another group of kapok cellulose from which lignin was removed was added into a NaOH / urea solution at -15 °C and stirred to obtain another transparent and uniform cellulose solution.
[0018] (4) The two cellulose solutions in step (3) are uniformly mixed in a mechanical dispersion device and reacted for a certain time within a certain temperature and pH range.
[0019] (5) The product of step (4) is precipitated, washed, and dried to obtain a nano ZnO / delignified kapok cellulose composite material.
[0020] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (1), the concentration of the ZnCl2 aqueous solution is 50 wt%, and the concentration of the NaOH / urea solution is 10 / 15 wt%.
[0021] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (3), the temperature at which cellulose is dissolved in the ZnCl2 solution is 90°C.
[0022] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the mechanical dispersion device is a colloid mill.
[0023] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (4), the reaction temperature of the two cellulose solutions is 45°C.
[0024] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the pH value of the reaction system is 13.
[0025] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the reaction time is 40 min. Example 2
[0026] (1) Prepare a mixed solution of sodium hydroxide and sodium sulfide, add it to kapok fiber and react it at 100 °C for 2 hours to remove most of the lignin in the kapok fiber.
[0027] (2) After washing and filtering, the excess water is dried, the kapok fiber is bleached with sodium hypochlorite to remove residual lignin, and then washed and dried.
[0028] (3) The kapok cellulose from which lignin was removed was added into a ZnCl2 solution at a certain temperature and stirred to obtain a transparent and uniform cellulose solution. At the same time, another group of kapok cellulose from which lignin was removed was added into a NaOH / urea solution at -15 °C and stirred to obtain another transparent and uniform cellulose solution.
[0029] (4) The two cellulose solutions in step (3) are uniformly mixed in a mechanical dispersion device and reacted for a certain time within a certain temperature and pH range.
[0030] (5) The product of step (4) is precipitated, washed and dried to obtain a nano ZnO / delignified kapok cellulose composite material. The size distribution of ZnO in the composite material can be referred to Figure 1 shown.
[0031] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (1), the concentration of the ZnCl2 aqueous solution is 60 wt%, and the concentration of the NaOH / urea solution is 10 / 15 wt%.
[0032] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in step (3), the temperature at which cellulose is dissolved in the ZnCl2 solution is 100°C.
[0033] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the mechanical dispersion device can be a colloid mill, a homogenizer, etc.
[0034] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the reaction temperature of the two cellulose solutions is 60°C.
[0035] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the pH value of the reaction system is 9.
[0036] According to a technical solution of a nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, in the step (4), the reaction time value is 60 min.
[0037] Although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention, and any modification using the inventive concept is included in the scope of patent protection.
Claims
1. A nano ZnO / delignified kapok cellulose composite material and a preparation method thereof, characterized in that: The following steps are involved: (1) preparing a mixed solution of sodium hydroxide and sodium sulfide, adding kapok fibers to the solution and reacting to remove most of the lignin in the kapok fibers; (2) After washing and filtering, the excess water is dried, the kapok fiber is bleached with sodium hypochlorite to remove residual lignin, and then washed and dried; (3) Adding the delignified kapok cellulose to a ZnCl2 solution at a certain temperature and stirring to obtain a transparent and uniform cellulose solution, while adding another group of delignified kapok cellulose to a low-temperature NaOH / urea solution and stirring to obtain another transparent and uniform cellulose solution; (4) uniformly mixing the two cellulose solutions in step (3) in a mechanical dispersion device and reacting them for a certain time within a certain temperature and pH range; (5) The product of step (4) is precipitated, washed, and dried to obtain a nano ZnO / delignified kapok cellulose composite material.
2. The nano ZnO / delignified kapok cellulose composite material and preparation method thereof according to claim 1, characterized in that: In the step (1), the concentration of the ZnCl2 aqueous solution is 50-60 wt%, and the concentration of the NaOH / urea solution is 10 / 15 wt%.
3. The nano ZnO / delignified kapok cellulose composite material and preparation method thereof according to claim 1, characterized in that: In step (3), the temperature at which cellulose is dissolved in the ZnCl2 solution is 90-100°C.
4. The nano ZnO / delignified kapok cellulose composite material and preparation method thereof according to claim 1, characterized in that: The cellulose in step (3) refers to the cellulose obtained after the original kapok fiber is subjected to delignification treatment.
5. The nano ZnO / delignified kapok cellulose composite material and preparation method thereof according to claim 1, characterized in that: In the step (4), the mechanical dispersing device is a colloid mill, a homogenizer, etc.
6. The nano ZnO / delignified kapok cellulose composite material and preparation method thereof according to claim 1, characterized in that: In the step (4), the reaction temperature of the two cellulose solutions is 45-60°C.
7. The nano ZnO / delignified kapok cellulose composite material and preparation method thereof according to claim 1, characterized in that: In the step (4), the reaction time is 40-60 min.