Preparation method and application of all-inorganic perovskite nanocrystalline composite cellulose material
By introducing cellulose into perovskite materials, a high-stability all-inorganic perovskite nanocrystal composite material is formed, which solves the problem of poor long-term stability of perovskite humidity sensors and realizes a high sensitivity and fast response humidity sensor.
Patent Information
- Application Number
- CN202311305301.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-09
- Publication Date
- 2024-12-03
AI Technical Summary
Perovskite materials have poor long-term stability in humidity sensors, especially the high solubility of CsPbBr3 NCs in water, which leads to easily damage to the structure, limiting their practical application.
The preparation method of all-inorganic perovskite nanocrystal composite cellulose material is adopted, and CsPbBr3 NCs are synthesized by thermal injection method, and cellulose is introduced to improve its morphology and stability. The porous structure of cellulose encapsulates CsPbBr3 NCs to form high stability composite material.
The high stability, reversibility and repeatability of all-inorganic perovskite nanocrystal composite cellulose materials are achieved. The humidity sensor prepared based on this has the advantages of high sensitivity, rapid response and long-term operation.
Smart Images

Figure CN119060414A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic semiconductor materials, and specifically relates to a preparation method and application of an all-inorganic perovskite nanocrystalline composite cellulose material. Background Art
[0002] With the development of science and technology, the process of informatization, digitization and intelligence in modern society is constantly advancing, and the demand for sensing and measurement and control devices is increasing. As one of the main means of obtaining information from the environment, how to improve the sensing performance of sensors has become a hot issue, and the selection of sensitive materials is a key link.
[0003] Perovskite is a crystalline material with a molecular formula of ABX3 and an octahedral shape, where A is a larger cation, such as the organic cation methylamine (MA + ), formamidine (FA + ), cesium metal ions (Cs + ) etc.; B is generally a divalent metal cation, such as lead ion (Pb 2+ ), tin ions (Sn 2+ ); X is generally a halogen anion, often Cl - Br - ,I - Each A ion is surrounded by an octahedron formed by B and X ions. According to the composition of A, it can be divided into two categories: organic-inorganic hybrid perovskite and all-inorganic perovskite.
[0004] Compared with organic-inorganic hybrid perovskites, due to the Cs + With the right size to occupy the A position, all-inorganic perovskites have higher thermal stability. In 2015, Kovalenko et al. reported the preparation of all-inorganic halide perovskite CsPbX3. In the following years, inorganic perovskite materials attracted a large number of researchers due to their excellent performance. Lead halide perovskites have made great progress in photodiodes, photodetectors, photoelectric sensors, laser devices, etc. due to their directly adjustable band gap, strong light absorption ability, good carrier transport characteristics, full spectrum tunability and high fluorescence quantum yield. Perovskite-based solar cells have also quickly occupied a place in the photovoltaic industry with their huge advantages of high conversion efficiency and low cost, promoting the development of photovoltaic technology.
[0005] The ultra-sensitive properties of metal halide perovskites to the environment are fully utilized. The advantages of high room temperature carrier migration rate, highly sensitive surface properties to the environment, simple preparation and cost-effectiveness make halide perovskites a potential choice for humidity-sensitive materials. Humidity-sensitive materials adsorb or desorb water molecules through changes in the water vapor content in the environment, thereby causing changes in their resistance or capacitance to quantitatively analyze humidity. The application of perovskite materials in humidity sensors cleverly transforms their disadvantage of instability in humidity environments into the advantage of high sensitivity of humidity sensors.
[0006] Humidity sensors are the most widely used type of sensors in human social life and industrial production, such as medical monitoring, smart agricultural monitoring, precise industrial process control, food storage environment monitoring, smart home and meteorological monitoring. However, the process of monitoring humidity will inevitably be affected by other factors in the environment, such as temperature, gas pressure, etc. Therefore, researchers have been committed to developing high-performance humidity sensors with good stability. In 2019, Weng et al. proposed a humidity sensor based on the Cs2BiAgBr6 double perovskite structure, which combines the unique humidity-sensitive properties of perovskite with good stability, providing a new path for the new application of perovskite. All-inorganic perovskite materials are expected to shine in the field of humidity sensing.
[0007] Although perovskite-based humidity sensors have excellent performance in all aspects, due to the ionic properties of CsPbBr3 NCs (nanocrystals) and the high solubility of CsBr in water, the structure of CsPbBr3 NCs is easily destroyed when exposed to water and converted into CsPb2Br5 NCs. Therefore, the long-term stability of perovskite materials is still the primary problem limiting its practical application. Summary of the invention
[0008] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing an all-inorganic perovskite nanocrystal composite cellulose material and its application. The all-inorganic perovskite nanocrystal composite cellulose material prepared by the method has good reversibility and repeatability. The humidity sensor based on the all-inorganic perovskite nanocrystal composite cellulose material has the advantages of simple preparation, high sensitivity and rapid response, and high stability in long-term operation, thereby solving the problem of poor long-term working stability of humidity sensors based on perovskite materials.
[0009] To achieve the above-mentioned purpose, the technical solution adopted by the present invention to solve the technical problem is: to provide a method for preparing an all-inorganic perovskite nanocrystalline composite cellulose material, comprising the following steps:
[0010] (1) under vacuum conditions, cesium carbonate, octadecene and oleic acid are mixed and calcined at 100-120° C. for 60-80 min, and then the temperature is raised to 140-160° C. until cesium carbonate and oleic acid react completely to obtain a cesium oleate solution;
[0011] (2) under vacuum conditions, mixing lead bromide and octadecene, and calcining at 100-120° C. for 60-80 min to obtain a lead bromide precursor solution;
[0012] (3) injecting oleic acid and oleylamine into the lead bromide precursor solution obtained in step (2) under ambient conditions, then calcining under vacuum conditions at 170-190° C. until the lead bromide is completely dissolved, then adding cellulose, and stirring at a constant rate for 60-90 minutes to obtain a lead bromide precursor / cellulose composite material;
[0013] (4) Under ambient conditions, injecting the cesium oleate solution obtained in step (1) into the lead bromide precursor / cellulose composite material obtained in step (3), centrifuging, and obtaining an all-inorganic perovskite nanocrystal composite cellulose material.
[0014] Furthermore, in step (1), the mass volume ratio of cesium carbonate, octadecene and oleic acid is 0.2-0.4 g:18-23 mL:1.0-1.5 mL.
[0015] Furthermore, in step (2), the mass volume ratio of lead bromide to octadecene is 0.05-0.06 g:4-6 mL.
[0016] Furthermore, in step (3), the mass volume ratio of the added cellulose, oleic acid and oleylamine is 0.04-0.06 g: 0.4-0.6 mL: 0.4-0.6 mL.
[0017] Furthermore, in step (4), the volume ratio of the cesium oleate injection volume to the lead bromide precursor / cellulose composite material is 0.4-0.6 mL:4.8-7.2 mL.
[0018] The present invention also provides an all-inorganic perovskite nanocrystal composite cellulose material prepared by the preparation method of the all-inorganic perovskite nanocrystal composite cellulose material.
[0019] The present invention also provides the use of the all-inorganic perovskite nanocrystal composite cellulose material in the preparation of a humidity sensor.
[0020] The present invention also provides a humidity sensor, comprising the above-mentioned all-inorganic perovskite nanocrystal composite cellulose material and interdigital electrodes.
[0021] The present invention also provides a method for preparing the humidity sensor, comprising the following steps:
[0022] (1) The interdigital electrode was ultrasonically cleaned in ethanol and deionized water for 10-30 min respectively, and then dried at 50-70° C. for 40-80 min;
[0023] (2) Fixing the wires to the dried interdigital electrodes with conductive silver paste and curing at 130-150° C. for 50-70 min;
[0024] (3) adding the all-inorganic perovskite nanocrystal composite cellulose material into a solvent and performing ultrasonication for 20-40 minutes to obtain a suspension;
[0025] (4) Using the drop coating method, 40-60 uL of the suspension obtained in step (3) is dropped drop by drop on the electrode, and then dried at 50-70° C. for 20-40 min to obtain a humidity sensor.
[0026] Furthermore, in step (3), the solvent is deionized water, n-hexane or dimethyl sulfoxide.
[0027] Furthermore, in step (3), the ratio of the all-inorganic perovskite nanocrystalline composite cellulose material to the solvent is 0.1-0.13 g:10 mL.
[0028] In summary, the present invention has the following advantages:
[0029] 1. This technology uses the hot injection method to synthesize perovskite nanocrystals (CsPbBr3 NCs). Since there are no metastable perovskite impurities in the synthesis process, the CsPbBr3 NCs synthesized by the hot injection method have fewer surface defects and better stability. The morphology of CsPbBr3 NCs is improved by introducing cellulose. After adding cellulose to the CsPbBr3 precursor solution, the viscosity of the precursor solution increases and the oxygen functional groups of cellulose react with the Pb in the precursor solution. 2+ interaction, passivating the uncoordinated Pb 2+ , and at the same time, the crystallization rate of CsPbBr3 NCs is reduced, giving them enough time to form a perovskite crystal structure with large grain size and low defect density, resulting in highly stable CsPbBr3 NCs. Due to the capillary action of cellulose, PbBr2 is spontaneously adsorbed and wrapped between rigid fibers, and CsPbBr3 NCs are nucleated through supersaturation of the precursor, so a large number of CsPbBr3 NCs are well wrapped in the porous structure of cellulose fibers and have high aggregation.
[0030] 2. Cellulose fibers have hydrophilic functional groups hydroxyl (-OH), carboxyl (-COOH) and highly porous network structures. Its hydrophilicity and porosity provide high sensitivity and rapid response to humidity. At the same time, the porous structure of cellulose provides a closed space, which confines the CsBr dissociated after CsPbBr3 NCs absorbs water. Once the water is removed, CsBr reacts with the residual CsPb2Br5 NCs to regenerate CsPbBr3NCs. Therefore, the prepared all-inorganic perovskite nanocrystal composite cellulose material (CsPbBr3 NCs / Cellulose) has good reversibility and repeatability.
[0031] 3. The CsPbBr3 in the composite material of the present invention is nano-sized, has a large specific surface area, is highly sensitive to humidity changes, and the sensitive film formed by regular nano-sized crystals enables the charge to migrate effectively in water vapor. In addition, the addition of cellulose having hydrophilic functional groups hydroxyl (-OH), carboxyl (-COOH) and a highly porous network structure further improves the response speed and sensitivity of the material to humidity.
[0032] 4. The CsPbBr3 NCs / Cellulose composite material prepared in the present invention has the advantages of high sensitivity to humidity, rapid response, high stability and reversibility and repeatability. The sensor using the CsPbBr3 NCs / Cellulose composite material as the humidity sensitive layer in the present invention has the characteristics of high sensitivity, rapid response and high stability in long-term operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The XRD spectrum of the all-inorganic perovskite nanocrystal composite cellulose material of the present invention; DETAILED DESCRIPTION
[0034] Example 1
[0035] A method for preparing an all-inorganic perovskite nanocrystalline composite cellulose material comprises the following steps:
[0036] (1) 0.2 g of cesium carbonate, 18 mL of octadecene and 1.0 mL of oleic acid were mixed under vacuum conditions, calcined in a vacuum drying oven at 100° C. for 60 min, and then heated to 140° C. until cesium carbonate and oleic acid reacted completely to obtain a cesium oleate solution;
[0037] (2) mixing 0.05 g of lead bromide and 4 mL of octadecene under vacuum conditions, and calcining in a vacuum drying oven at 100° C. for 60 min to obtain a lead bromide precursor solution;
[0038] (3) Under ambient conditions, injecting 0.4 mL of oleic acid and 0.4 mL of oleylamine into the lead bromide precursor solution obtained in step (2), then calcining in a vacuum drying oven at 170° C. until the lead bromide is completely dissolved, adding 0.04 g of cellulose, and stirring at a constant rate for 60 min to obtain a lead bromide precursor / cellulose composite material;
[0039] (4) Under ambient conditions, injecting 0.4 mL of the cesium oleate solution obtained in step (1) into the lead bromide precursor / cellulose composite material obtained in step (3), and centrifuging to obtain an all-inorganic perovskite nanocrystal composite cellulose material.
[0040] Example 2
[0041] A method for preparing an all-inorganic perovskite nanocrystalline composite cellulose material comprises the following steps:
[0042] (1) 0.4 g of cesium carbonate, 23 mL of octadecene and 1.5 mL of oleic acid were mixed under vacuum conditions, calcined in a vacuum drying oven at 120° C. for 80 min, and then heated to 160° C. until cesium carbonate and oleic acid reacted completely to obtain a cesium oleate solution;
[0043] (2) mixing 0.06 g of lead bromide and 6 mL of octadecene under vacuum conditions, and calcining in a vacuum drying oven at 120° C. for 80 min to obtain a lead bromide precursor solution;
[0044] (3) Under ambient conditions, injecting 0.6 mL of oleic acid and 0.6 mL of oleylamine into the lead bromide precursor solution obtained in step (2), then calcining in a vacuum drying oven at 190° C. until the lead bromide is completely dissolved, adding 0.06 g of cellulose, and stirring at a constant rate for 90 min to obtain a lead bromide precursor / cellulose composite material;
[0045] (4) Under ambient conditions, injecting 0.6 mL of the cesium oleate solution obtained in step (1) into the lead bromide precursor / cellulose composite material obtained in step (3), and centrifuging to obtain an all-inorganic perovskite nanocrystal composite cellulose material.
[0046] Example 3
[0047] A method for preparing an all-inorganic perovskite nanocrystalline composite cellulose material comprises the following steps:
[0048] (1) 0.326 g of cesium carbonate, 20 mL of octadecene and 1.25 mL of oleic acid were mixed under vacuum conditions, calcined in a vacuum drying oven at 110° C. for 70 min, and then heated to 150° C. until cesium carbonate and oleic acid reacted completely to obtain a cesium oleate solution;
[0049] (2) mixing 0.058 g of lead bromide and 5 mL of octadecene under vacuum conditions, and calcining in a vacuum drying oven at 110° C. for 70 min to obtain a lead bromide precursor solution;
[0050] (3) under ambient conditions, injecting 0.5 mL of oleic acid and 0.5 mL of oleylamine into the lead bromide precursor solution obtained in step (2), then calcining in a vacuum drying oven at 185° C. until the lead bromide is completely dissolved, adding 0.05 g of cellulose, and stirring at a constant rate for 80 min to obtain a lead bromide precursor / cellulose composite material;
[0051] (4) Under ambient conditions, injecting 0.5 mL of the cesium oleate solution obtained in step (1) into the lead bromide precursor / cellulose composite material obtained in step (3), and centrifuging to obtain an all-inorganic perovskite nanocrystal composite cellulose material.
[0052] Example 4
[0053] A method for manufacturing a humidity sensor comprises the following steps:
[0054] (1) The interdigitated electrode was ultrasonically cleaned in ethanol and deionized water for 10 min respectively, and then the electrode was dried at 50 °C for 40 min;
[0055] (2) Fix the wires to the dried interdigital electrodes with conductive silver paste and cure at 130°C for 50 min;
[0056] (3) 0.1 g of the all-inorganic perovskite nanocrystalline composite cellulose material obtained in Example 3 was added to 10 mL of deionized water and ultrasonicated for 20 min to obtain a suspension;
[0057] (4) Using the drop coating method, 40 uL of the suspension obtained in step (3) was dropped drop by drop on the electrode, and then dried at 50° C. for 20 min to obtain a humidity sensor.
[0058] Example 5
[0059] A method for manufacturing a humidity sensor comprises the following steps:
[0060] (1) The interdigitated electrode was ultrasonically cleaned in ethanol and deionized water for 30 min respectively, and then the electrode was dried at 70 °C for 80 min;
[0061] (2) Fix the wires to the dried interdigital electrodes with conductive silver paste and cure at 150°C for 70 min;
[0062] (3) adding 0.13 g of the all-inorganic perovskite nanocrystalline composite cellulose material obtained in Example 3 to 10 mL of n-hexane and performing ultrasonication for 40 min to obtain a suspension;
[0063] (4) Using the drop coating method, 60 uL of the suspension obtained in step (3) was dripped drop by drop on the electrode, and then dried at 70° C. for 40 min to obtain a humidity sensor.
[0064] Example 6
[0065] 8. The method for manufacturing the humidity sensor according to claim 7, characterized in that it comprises the following steps:
[0066] (1) The interdigitated electrode was ultrasonically cleaned in ethanol and deionized water for 20 min respectively, and then the electrode was dried at 60 °C for 60 min;
[0067] (2) Fix the wires to the dried interdigital electrodes with conductive silver paste and cure at 140°C for 60 min;
[0068] (3) adding 0.116 g of all-inorganic perovskite nanocrystal composite cellulose material into 10 mL of dimethyl sulfoxide and performing ultrasonication for 30 min to obtain a suspension;
[0069] (4) Using the drop coating method, 50 uL of the suspension obtained in step (3) was dropped drop by drop on the electrode, and then dried at 60° C. for 30 min to obtain a humidity sensor.
[0070] Experimental Example 1
[0071] The all-inorganic perovskite nanocrystalline composite cellulose material obtained in Example 3 was subjected to XRD, and its spectrum is as follows: Figure 1 As shown, from top to bottom are the spectra of cellulose (Cellulose) and all-inorganic perovskite nanocrystal composite cellulose material (CsPbBr3 NCs / Cellulose).
[0072] Depend on Figure 1 It can be seen that the CsPbBr3 NCs / Cellulose composite material has clear diffraction peaks at 15.02°, 21.34°, and 30.24°, which correspond to the (100), (110), and (200) planes of the α-phase CsPbBr3 perovskite crystal, respectively, and are consistent with the cubic crystal structure of CsPbBr3 (PDF#97-002-9073). In addition, the diffraction peak of the CsPbBr3 NCs / Cellulose composite material at 22.43° corresponds to the diffraction peak of commercial cellulose, proving the successful composite of the prepared CsPbBr3 NCs and Cellulose.
[0073] In summary, the present invention adopts the hot injection method to synthesize perovskite nanocrystals (CsPbBr3 NCs). Since there are no metastable perovskite impurities in the synthesis process, the CsPbBr3 NCs synthesized by the hot injection method have few surface defects and good stability. By introducing cellulose, a perovskite crystal structure with large grain size and low defect density is formed, and highly stable CsPbBr3 NCs are obtained. CsPbBr3 NCs are well wrapped in the porous structure of cellulose fibers and have high aggregation. Cellulose fibers have hydrophilic functional groups hydroxyl (-OH), carboxyl (-COOH) and a highly porous mesh structure. Its hydrophilicity and porosity provide high sensitivity and rapid response to humidity. At the same time, the porous structure of cellulose provides a closed space, which confines the CsBr dissociated after CsPbBr3NCs absorbs water. Once the water is removed, CsBr reacts with the residual CsPb2Br5NCs to regenerate CsPbBr3NCs, making the all-inorganic perovskite nanocrystal composite cellulose material (CsPbBr3NCs / Cellulose) have good reversibility and repeatability. The humidity sensor made based on the CsPbBr3NCs / Cellulose composite material has the advantages of simple preparation, high sensitivity, rapid response and high stability in long-term operation.
[0074] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.
Claims
1. A method for preparing an all-inorganic perovskite nanocrystal composite cellulose material, characterized in that: The following steps are involved: (1) under vacuum conditions, cesium carbonate, octadecene and oleic acid are mixed and calcined at 100-120° C. for 60-80 min, and then the temperature is raised to 140-160° C. until cesium carbonate and oleic acid react completely to obtain a cesium oleate solution; (2) under vacuum conditions, mixing lead bromide and octadecene, and calcining at 100-120° C. for 60-80 min to obtain a lead bromide precursor solution; (3) injecting oleic acid and oleylamine into the lead bromide precursor solution obtained in step (2) under ambient conditions, then calcining under vacuum conditions at 170-190° C. until the lead bromide is completely dissolved, then adding cellulose, and stirring at a constant rate for 60-90 minutes to obtain a lead bromide precursor / cellulose composite material; (4) Under ambient conditions, injecting the cesium oleate solution obtained in step (1) into the lead bromide precursor / cellulose composite material obtained in step (3), centrifuging, and obtaining an all-inorganic perovskite nanocrystal composite cellulose material.
2. The method for preparing the all-inorganic perovskite nanocrystalline composite cellulose material according to claim 1, characterized in that: In step (1), the mass volume ratio of cesium carbonate, octadecene and oleic acid is 0.2-0.4 g:18-23 mL:1.0-1.5 mL.
3. The method for preparing the all-inorganic perovskite nanocrystalline composite cellulose material according to claim 1, characterized in that: In step (2), the mass volume ratio of lead bromide to octadecene is 0.05-0.06 g:4-6 mL.
4. The method for preparing the all-inorganic perovskite nanocrystalline composite cellulose material according to claim 1, characterized in that: In step (3), the mass volume ratio of the added cellulose, oleic acid and oleylamine is 0.04-0.06 g: 0.4-0.6 mL: 0.4-0.6 mL.
5. The method for preparing the all-inorganic perovskite nanocrystalline composite cellulose material according to claim 1, characterized in that: In step (4), the volume ratio of the cesium oleate injection volume to the lead bromide precursor / cellulose composite material is 0.4-0.6 mL:4.8-7.2 mL.
6. The all-inorganic perovskite nanocrystal composite cellulose material obtained by the preparation method of the all-inorganic perovskite nanocrystal composite cellulose material according to any one of claims 1 to 5.
7. Use of the all-inorganic perovskite nanocrystal composite cellulose material according to claim 6 in the preparation of a humidity sensor.
8. A humidity sensor, characterized in that: It comprises the all-inorganic perovskite nanocrystalline composite cellulose material and interdigital electrodes as described in claim 6.
9. The method for preparing the humidity sensor according to claim 8, characterized in that: The following steps are involved: (1) The interdigital electrode was ultrasonically cleaned in ethanol and deionized water for 10-30 min respectively, and then dried at 50-70° C. for 40-80 min; (2) Fixing the wires to the dried interdigital electrodes with conductive silver paste and curing at 130-150° C. for 50-70 min; (3) adding the all-inorganic perovskite nanocrystal composite cellulose material into a solvent and performing ultrasonication for 20-40 minutes to obtain a suspension; (4) Using the drop coating method, 40-60 uL of the suspension obtained in step (3) is dropped drop by drop on the electrode, and then dried at 50-70° C. for 20-40 min to obtain a humidity sensor.
10. The method for preparing a humidity sensor according to claim 7, characterized in that: In step (3), the solvent is deionized water, n-hexane or dimethyl sulfoxide.