Modified starch as well as preparation method and application thereof

By radiating the starch and using multiple modification treatments, stable crosslinked copolymers and modified starch are formed, which solves the stability and cementitious performance of starch-type wood adhesives and achieves high stability of modified starch Properties and cement properties extend the service life of the wood.

CN119060418APending Publication Date: 2024-12-03JILIN TEACHERS INST OF ENG & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411349918.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing starch modification methods have problems such as safety hazards, high cost, reduced viscosity, and reduced adhesive capacity, starch-type wood adhesives are not water-resistant, easy to delaminate, and poor stability. They are especially prone to carbonization at high temperatures, which affects the service life of the wood. .

Method used

After irradiation of starch with 60Co-γ-ray, cross-linking with biphenyl chloride and aniline, oxidizing starch with polyurethaneimide, octenyl succinic anhydride and hydroxypropylation, a stable starch-linking is formed Benzoyl chloride-aniline crosslinking copolymer, polyurethane imide modified starch, octenyl succinic anhydride modified starch and hydroxypropylated modified starch improve their stability and cementitious properties.

Benefits of technology

The modified starch obtained has strong stability, is not easy to delaminate and has excellent cementing performance, extends the shelf life, avoids carbonization problems, and significantly improves the service life of wood adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005062054280000031
    Figure BDA0005062054280000031
  • Figure BDA0005062054280000032
    Figure BDA0005062054280000032
  • Figure BDA0005062054280000033
    Figure BDA0005062054280000033
Patent Text Reader

Abstract

The invention belongs to the technical field of starch modification methods, and particularly relates to modified starch as well as a preparation method and application thereof. The preparation method comprises the following steps: respectively preparing a starch-biphenyl chloride-aniline cross-linked copolymer, polyurethane imide modified starch, octenyl succinic anhydride modified starch and hydroxypropylation modified starch, and then mixing the starch-biphenyl chloride-aniline cross-linked copolymer, the polyurethane imide modified starch, the octenyl succinic anhydride modified starch and the hydroxypropylation modified starch together to prepare the modified starch. The modified starch prepared by the preparation method disclosed by the invention has better stability and cementing performance, is not easy to cake and layer, prolongs the storage period, avoids the problem of carbonization during use, improves the cementing capacity and the cementing efficiency, and can greatly prolong the service life of wood.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of starch modification methods, and specifically relates to modified starch and a preparation method and application thereof. Background Art

[0002] At present, the methods for modifying starch mainly include chemical methods (grafting, oxidation, esterification, etc.), physical methods (heat treatment, microwave treatment, irradiation treatment, etc.) and enzyme methods (glycosyltransferase, etc.). Although the above modification methods can reduce the viscosity of starch to a certain extent and improve its water holding capacity, they still have certain technical problems. For example, the chemical method uses chemical reagents, which has certain safety hazards and needs to be strictly followed; the physical method uses more instruments and equipment, and the cost is relatively high; the enzyme method reduces the starch viscosity while reducing the starch's ability to promote gel formation and thickening function.

[0003] When starch is made into wood adhesive, since starch is a natural crystalline substance, the presence of the crystalline region makes the wood adhesive made from starch not water-resistant, and the hydroxyl groups in the crystalline region can also lead to low adhesive ability and efficiency of the wood adhesive made from starch. Therefore, the presence of starch crystalline regions causes starch-based wood adhesives to have problems such as poor stability, easy delamination, unsatisfactory use effect, and poor bonding performance. In addition, when starch-based wood adhesives are used at temperatures above 120°C, the starch will carbonize for more than half an hour, thus affecting the service life of the wood. Summary of the invention

[0004] Therefore, in order to solve the technical problems existing in the existing starch modification methods and provide a starch-based wood adhesive with strong stability, low stratification and strong bonding performance, the present invention provides a modified starch and a preparation method and application thereof.

[0005] The technical solution adopted by the present invention to solve the technical problem is as follows:

[0006] The present invention provides a method for preparing modified starch, which specifically comprises the following steps:

[0007] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0008] After irradiating the starch under a 60Co-γ-ray irradiation source, a strong acid solution is added and stirred to fully mix, and then diphenyl chloride and aniline are added for cross-linking reaction, and after ultrasonic treatment, a sodium hydroxide solution is slowly added dropwise to adjust the pH to 4-6 to obtain a starch-diphenyl chloride-aniline cross-linked copolymer;

[0009] (2) preparing polyurethane imide modified starch;

[0010] First, an oxidant is added to starch to obtain oxidized starch, and then the oxidized starch, polyurethane imide, glycerol and acetone solution are uniformly mixed, and then reacted in a constant temperature water bath of 85°C-95°C for 1.5h-2.5h. After the reaction is completed, the temperature is lowered to a constant temperature water bath of 60°C-80°C for 0.5h-1h to obtain polyurethane imide modified starch;

[0011] (3) preparing octenyl succinic anhydride modified starch;

[0012] After the starch and octenyl succinic anhydride are uniformly mixed, the mixture is reacted in a constant temperature water bath at 55°C-60°C for 1.5h-2.5h, and after ultrasonic treatment, a sodium hydroxide solution is slowly added dropwise to adjust the pH to 4-6 to obtain octenyl succinic anhydride modified starch;

[0013] (4) preparing hydroxypropyl modified starch;

[0014] Add polyamine compound, carboxymethyl chitosan and hydroxypropyl chitosan in a mass ratio of (0.5-1.5): (1.3-2.1): (1.4-1.9) to a weak acid solution, stir evenly, add twice the weight of starch, and react in a constant temperature water bath at 40°C-50°C for 1h-2h to obtain hydroxypropyl modified starch;

[0015] (5) preparing modified starch;

[0016] The obtained starch-biphenyl chloride-aniline cross-linked copolymer, polyurethane imide modified starch, octenyl succinic anhydride modified starch and hydroxypropyl modified starch were placed in an oven at 40°C-50°C in a mass ratio of (4-10):(5-10):(7-15):(5-15), and then crushed, sieved and mixed to obtain a modified starch sample.

[0017] Preferably, in steps (1) to (4), the starch is selected from one of corn starch, mung bean starch, sweet potato starch, cassava starch, sweet potato starch, water chestnut starch, wheat starch, potato starch, and lotus root starch.

[0018] Preferably, in step (1) and step (3), the frequency of the ultrasonic treatment is 25kHz-35kHz, and the time is 40min-100min.

[0019] Preferably, in step (1), the mass ratio of starch, benzyl chloride and aniline is (0.4-1.6):(1.7-2.6):(1.0-2.5).

[0020] Preferably, in step (1), the biphenyl chloride is selected from 2,2′,4,4′-biphenyl tetrachloride, 2,2′,5,5′-biphenyl tetrachloride, 3,3′,5,5′-biphenyl tetrachloride, 2,3′,4,5′,6,-biphenyl pentachloride or 2,2′,4,4′,6,6′-biphenyl hexachloride;

[0021] The structural formula of the 2,2′,4,4′-biphenyltetraacyl chloride is:

[0022]

[0023] The structural formula of the 2,2′,5,5′-biphenyltetraacyl chloride is:

[0024]

[0025] The structural formula of the 3,3′,5,5′-biphenyltetraacyl chloride is:

[0026]

[0027] The structural formula of the 2,3′,4,5′,6-biphenylpentachloride is:

[0028]

[0029] The structural formula of the 2,2′,4,4′,6,6′-biphenylhexachloride is:

[0030]

[0031] Preferably, in step (1), the strong acid solution is selected from a sulfuric acid solution, a nitric acid solution, and a hydrochloric acid solution.

[0032] Preferably, in step (4), the weak acid solution is selected from acetic acid and hydrofluoric acid.

[0033] Preferably, in step (2), the oxidant is selected from one of sodium hypochlorite, hydrogen peroxide, sodium sulfate, ammonium persulfate, and potassium permanganate.

[0034] Preferably, in step (4), the polyamine compound has a structure of formula (I), formula (II) or formula (III):

[0035]

[0036] Where m = 2-10, n = 2-10;

[0037]

[0038] Where R = C 11 H 23, n = 9;

[0039]

[0040] Among them, n=16.

[0041] The invention provides modified starch prepared by the modified starch preparation method.

[0042] The invention provides application of the modified starch prepared by the modified starch preparation method in preparing wood adhesive.

[0043] The beneficial effects of the present invention are:

[0044] In a preparation method of modified starch provided by the present invention, when preparing a starch-biphenylyl chloride-aniline cross-linked copolymer, the starch is pre-denatured by irradiation, and then a strong acid solution is used to fully dissolve the pre-denatured starch to convert starch macromolecules into monomer starch molecules, and then biphenylyl chloride and aniline are added for cross-linking reaction, and the monomer starch molecules are connected and cross-linked by the cross-linking effect of the biphenylyl chloride and aniline to obtain the starch-biphenylyl chloride-aniline cross-linked copolymer. The stability and bonding performance of the starch-biphenylyl chloride-aniline cross-linked copolymer can be improved by the cross-linking effect of the biphenylyl chloride and aniline, and the copolymer is not easy to be delaminated and agglomerated, and the carbonization problem is solved at the same time, which is convenient for subsequent use.

[0045] In a preparation method of modified starch provided by the present invention, when preparing polyurethane imide modified starch, an oxidant is first added to the starch for pre-denaturation, and then the oxidized starch, polyurethane imide, glycerol and acetone solution are evenly mixed and reacted in a constant temperature water bath, and the pre-denatured oxidized starch is modified again by polyurethane imide, and glycerol and acetone are added at the same time to make the starch dispersed more evenly and improve the reaction efficiency. The starch modified by polyurethane imide has improved bonding ability and adhesive efficiency, and the stratification and agglomeration problems are solved due to good dispersibility.

[0046] In a preparation method of modified starch provided by the present invention, when preparing octenyl succinic anhydride modified starch, starch and octenyl succinic anhydride are mixed and then reacted in a constant temperature water bath, and sodium hydroxide solution is slowly added dropwise after ultrasonic treatment to adjust the pH value, so as to obtain octenyl succinic anhydride modified starch. The starch is directly modified by octenyl succinic anhydride, so that the stability of the starch can be improved, and the starch is not easy to be delaminated, thereby increasing the storage time.

[0047] In a preparation method of modified starch provided by the present invention, when preparing hydroxypropyl modified starch, polyamine compound, carboxymethyl chitosan and hydroxypropyl chitosan are added to a weak acid solution, and then starch is added to react in a constant temperature water bath to obtain hydroxypropyl modified starch. The combined action of polyamine compound, carboxymethyl chitosan and hydroxypropyl chitosan can improve the stability of starch, make starch less likely to stratify, and increase the storage time.

[0048] In a preparation method of modified starch provided by the present invention, when preparing the modified starch, the obtained starch-biphenylyl chloride-aniline cross-linked copolymer, polyurethane imide modified starch, octenyl succinic anhydride modified starch and hydroxypropyl modified starch are placed in an oven for drying, and then crushed, sieved and mixed to obtain a modified starch sample. Since each starch is modified, the modified starch finally obtained has excellent storage performance, strong stability, long storage period, greatly improved bonding performance, and at the same time improves the carbonization problem existing in the existing modified starch, which can greatly improve the service life of the wood. DETAILED DESCRIPTION

[0049] The present invention provides a method for preparing modified starch, which specifically comprises the following steps:

[0050] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0051] After irradiating starch under a 60Co-γ-ray irradiation source, a strong acid solution is added and stirred to make it fully mixed, and then benzyl chloride and aniline are added for cross-linking reaction, wherein the mass ratio of starch, benzyl chloride and aniline is (0.4-1.6): (1.7-2.6): (1.0-2.5), and after ultrasonic treatment at a frequency of 25kHz-35kHz for 40min-100min, a sodium hydroxide solution is slowly added dropwise to adjust the pH to 4-6 to obtain a starch-benzyl chloride-aniline cross-linked copolymer.

[0052] The starch is selected from one of corn starch, mung bean starch, sweet potato starch, cassava starch, sweet potato starch, water chestnut starch, wheat starch, potato starch, and lotus root starch, but is not limited thereto.

[0053] The strong acid solution is selected from sulfuric acid solution, nitric acid solution and hydrochloric acid solution, but is not limited thereto.

[0054] The biphenyl chloride is selected from 2,2′,4,4′-biphenyl tetrachloride, 2,2′,5,5′-biphenyl tetrachloride, 3,3′,5,5′-biphenyl tetrachloride, 2,3′,4,5′,6,-biphenyl pentachloride or 2,2′,4,4′,6,6′-biphenyl hexachloride, but is not limited thereto.

[0055] Among them, the structural formula of 2,2′,4,4′-biphenyltetraacyl chloride is as follows:

[0056]

[0057] Among them, the structural formula of 2,2′,5,5′-biphenyltetrachloride is as follows:

[0058]

[0059] Among them, the structural formula of 3,3′,5,5′-biphenyltetraacyl chloride is:

[0060]

[0061] Among them, the structural formula of 2,3′,4,5′,6-biphenylpentachloride is as follows:

[0062]

[0063] Among them, the structural formula of 2,2′,4,4′,6,6′-biphenylhexachloride is as follows:

[0064]

[0065] (2) preparing polyurethane imide modified starch;

[0066] First, an oxidant is added to starch to obtain oxidized starch, and then the oxidized starch, polyurethane imide, glycerol and acetone solution are evenly mixed, and reacted in a constant temperature water bath of 85°C-95°C for 1.5h-2.5h. After the reaction, the temperature is lowered to 60°C-80°C and reacted in a constant temperature water bath for 0.5h-1h to obtain polyurethane imide modified starch.

[0067] The starch is selected from one of corn starch, mung bean starch, sweet potato starch, cassava starch, sweet potato starch, water chestnut starch, wheat starch, potato starch, and lotus root starch, but is not limited thereto.

[0068] The oxidant is selected from sodium hypochlorite, hydrogen peroxide, sodium sulfate, ammonium persulfate, and potassium permanganate, but is not limited thereto.

[0069] (3) preparing octenyl succinic anhydride modified starch;

[0070] After starch and octenyl succinic anhydride are uniformly mixed, reacted in a constant temperature water bath at 55°C-60°C for 1.5h-2.5h, ultrasonically treated at a frequency of 25kHz-35kHz for 40min-100min, and then slowly dripped with sodium hydroxide solution to adjust the pH to 4-6, to obtain octenyl succinic anhydride modified starch; wherein the starch is selected from one of corn starch, mung bean starch, sweet potato starch, cassava starch, sweet potato starch, water chestnut starch, wheat starch, potato starch, and lotus root starch, but not limited thereto.

[0071] (4) preparing hydroxypropyl modified starch;

[0072] Add polyamine compound, carboxymethyl chitosan and hydroxypropyl chitosan into a weak acid solution in a mass ratio of (0.5-1.5):(1.3-2.1):(1.4-1.9), stir evenly and add twice the weight of starch, react in a constant temperature water bath at 40°C-50°C for 1h-2h to obtain hydroxypropyl modified starch.

[0073] The starch is selected from one of corn starch, mung bean starch, sweet potato starch, cassava starch, sweet potato starch, water chestnut starch, wheat starch, potato starch, and lotus root starch, but is not limited thereto.

[0074] Wherein, the weak acid solution is selected from one of acetic acid and hydrofluoric acid, but is not limited thereto.

[0075] Wherein, the polyamine compound has the structure of formula (I), formula (II) or formula (III):

[0076]

[0077] Where m = 2-10, n = 2-10;

[0078]

[0079] Where R = C 11 H 23 , n = 9;

[0080]

[0081] Among them, n=16.

[0082] (5) preparing modified starch;

[0083] The obtained starch-biphenyl chloride-aniline cross-linked copolymer, polyurethane imide modified starch, octenyl succinic anhydride modified starch and hydroxypropyl modified starch were placed in an oven at 40°C-50°C in a mass ratio of (4-10):(5-10):(7-15):(5-15), and then crushed, sieved and mixed to obtain a modified starch sample.

[0084] The invention provides modified starch prepared by the modified starch preparation method.

[0085] The invention provides application of the modified starch prepared by the modified starch preparation method in preparing wood adhesive.

[0086] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0087] Example 1 Preparation of modified starch

[0088] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0089] 0.525 g corn starch was irradiated under a 60Co-γ-ray irradiation source for 3 h, and then a 0.5% nitric acid solution was added and stirred to be fully mixed, and then 2.051 g 3,3′,5,5′-biphenyltetrachloride and 1.101 g aniline were added for cross-linking reaction, and after ultrasonic treatment at a frequency of 32 kHz for 55 min, a 10% sodium hydroxide solution was slowly added dropwise to adjust the pH to 5, to obtain a starch-biphenyl chloride-aniline cross-linked copolymer;

[0090] (2) preparing polyurethane imide modified starch;

[0091] First, 0.254 g of sodium hypochlorite was added to 1.625 g of potato starch to obtain oxidized starch, and then 2.525 g of oxidized starch, 0.045 g of polyurethane imide, 20 ml of glycerol, and 100 ml of acetone solution were mixed evenly, and reacted in a constant temperature water bath at 90° C. for 2 h. After the reaction was completed, the temperature was lowered to 70° C. and reacted in a constant temperature water bath for 0.6 h to obtain polyurethane imide modified starch;

[0092] (3) preparing octenyl succinic anhydride modified starch;

[0093] 1.368 g corn starch and 0.784 g octenyl succinic anhydride were mixed evenly, reacted in a constant temperature water bath at 55°C for 2 h, and then ultrasonically treated at a frequency of 32 kHz for 55 min, and then sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain octenyl succinic anhydride modified starch;

[0094] (4) preparing hydroxypropyl modified starch;

[0095] 1.025 g of a polyamine compound having a structure of formula (I) (m=5, n=5), 1.589 g of carboxymethyl chitosan, and 1.527 g of hydroxypropyl chitosan were added to a 5% hydrofluoric acid solution, stirred evenly, and then 8.282 g of potato starch was added, and the mixture was reacted in a constant temperature water bath at 45° C. for 2 h to obtain a hydroxypropyl modified starch;

[0096] (5) preparing modified starch;

[0097] 8.14 g of starch-biphenylyl chloride-aniline cross-linked copolymer, 7.05 g of polyurethane imide modified starch, 9.21 g of octenyl succinic anhydride modified starch and 6.25 g of hydroxypropyl modified starch were placed in a 45°C oven for drying, crushed and mixed through an 80-mesh sieve to obtain a modified starch sample.

[0098] Example 2 Preparation of modified starch

[0099] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0100] After irradiating 1.6 g corn starch under a 60Co-γ-ray irradiation source for 3 h, a 0.5% hydrochloric acid solution was added and stirred to be fully mixed, and then 2.532 g 2,2′,5,5′-biphenyltetrachloride and 1.536 g aniline were added for cross-linking reaction, and after ultrasonic treatment at a frequency of 25 kHz for 45 min, a 10% sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain a starch-biphenyl chloride-aniline cross-linked copolymer;

[0101] (2) preparing polyurethane imide modified starch;

[0102] First, 0.265 g of sodium sulfate was added to 1.562 g of corn starch to obtain oxidized starch, and then 3.254 g of oxidized starch, 0.0954 g of polyurethane imide, 20 ml of glycerol, and 100 ml of acetone solution were mixed evenly, and reacted in a constant temperature water bath at 95° C. for 2 h. After the reaction was completed, the temperature was lowered to 75° C. and reacted in a constant temperature water bath for 0.5 h to obtain polyurethane imide modified starch;

[0103] (3) preparing octenyl succinic anhydride modified starch;

[0104] 1.877 g corn starch and 0.569 g octenyl succinic anhydride were mixed evenly, reacted in a constant temperature water bath at 60° C. for 2.5 h, and then ultrasonically treated at a frequency of 30 kHz for 60 min, and then sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain octenyl succinic anhydride modified starch;

[0105] (4) preparing hydroxypropyl modified starch;

[0106] 1.698 g of a polyamine compound having the structure of formula (I) (m=5, n=5), 2.056 g of carboxymethyl chitosan, and 1.458 g of hydroxypropyl chitosan were added to a 5% acetic acid solution, and after being stirred evenly, 10.424 g of corn starch was added, and the mixture was reacted in a constant temperature water bath at 48° C. for 1.8 h to obtain a hydroxypropyl modified starch;

[0107] (5) preparing modified starch;

[0108] 6.985 g of starch-biphenylyl chloride-aniline cross-linked copolymer, 6.874 g of polyurethane imide modified starch, 8.963 g of octenyl succinic anhydride modified starch and 10.54 g of hydroxypropyl modified starch were placed in a 50°C oven for drying, crushed and mixed through an 80-mesh sieve to obtain a modified starch sample.

[0109] Example 3 Preparation of modified starch

[0110] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0111] After irradiating 1.6 g corn starch under a 60Co-γ-ray irradiation source for 3 h, a 0.5% nitric acid solution was added and stirred to be fully mixed, and then 1.895 g 2,3′,4,5′,6,-biphenylpentachloride and 2.012 g aniline were added for cross-linking reaction, and after ultrasonic treatment at a frequency of 35 kHz for 75 min, a 10% sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain a starch-biphenyl chloride-aniline cross-linked copolymer;

[0112] (2) preparing polyurethane imide modified starch;

[0113] First, 0.457 g of ammonium persulfate was added to 1.775 g of potato starch to obtain oxidized starch, and then 3.541 g of oxidized starch, 0.57 g of polyurethane imide, 25 ml of glycerol, and 100 ml of acetone solution were mixed evenly, and reacted in a constant temperature water bath at 85° C. for 2 h. After the reaction was completed, the temperature was lowered to 65° C. and reacted in a constant temperature water bath for 1 h to obtain polyurethane imide modified starch;

[0114] (3) preparing octenyl succinic anhydride modified starch;

[0115] 1.487 g of potato starch and 0.963 g of octenyl succinic anhydride were mixed evenly, reacted in a constant temperature water bath at 60°C for 2.3 h, and then ultrasonically treated at a frequency of 28 kHz for 85 min, and then sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain octenyl succinic anhydride modified starch;

[0116] (4) preparing hydroxypropyl modified starch;

[0117] 1.50 g of a polyamine compound having a structure of formula (II), 1.354 g of carboxymethyl chitosan, and 1.458 g of hydroxypropyl chitosan were added to a 5% acetic acid solution, and after being stirred evenly, 8.624 g of corn starch was added, and the mixture was reacted in a constant temperature water bath at 50° C. for 1.5 h to obtain a hydroxypropyl modified starch;

[0118] (5) preparing modified starch;

[0119] 7.45 g of starch-biphenylyl chloride-aniline cross-linked copolymer, 5.69 g of polyurethane imide modified starch, 8.21 g of octenyl succinic anhydride modified starch and 7.18 g of hydroxypropyl modified starch were placed in a 50°C oven for drying, crushed and mixed through an 80-mesh sieve to obtain a modified starch sample.

[0120] Example 4 Preparation of modified starch

[0121] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0122] After irradiating 0.789 g of potato starch under a 60Co-γ-ray irradiation source for 3 h, a 0.5% sulfuric acid solution was added and stirred to be fully mixed, and then 3.54 g of 2,2′,4,4′,6,6′-biphenylhexachloride and 1.25 g of aniline were added for cross-linking reaction, and after ultrasonic treatment at a frequency of 25 kHz for 50 min, a 10% sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain a starch-biphenyl chloride-aniline cross-linked copolymer;

[0123] (2) preparing polyurethane imide modified starch;

[0124] First, 0.541 g of potassium permanganate was added to 1.734 g of potato starch to obtain oxidized starch, and then 2.7 g of oxidized starch, 0.048 g of polyurethane imide, 30 ml of glycerol, and 110 ml of acetone solution were mixed evenly, and reacted in a constant temperature water bath at 92° C. for 1.8 h. After the reaction was completed, the temperature was lowered to 65° C. and reacted in a constant temperature water bath for 0.9 h to obtain polyurethane imide modified starch;

[0125] (3) preparing octenyl succinic anhydride modified starch;

[0126] 1.536 g of potato starch and 0.896 g of octenyl succinic anhydride were mixed evenly, reacted in a constant temperature water bath at 60°C for 1.6 h, and then ultrasonically treated at a frequency of 26 kHz for 65 min, and then sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain octenyl succinic anhydride modified starch;

[0127] (4) preparing hydroxypropyl modified starch;

[0128] 0.95 g of a polyamine compound having a structure of formula (II), 1.478 g of carboxymethyl chitosan, and 1.498 g of hydroxypropyl chitosan were added to a 5% hydrofluoric acid solution, stirred evenly, and then 7.852 g of potato starch was added, and the mixture was reacted in a constant temperature water bath at 45° C. for 2 h to obtain a hydroxypropyl modified starch;

[0129] (5) preparing modified starch;

[0130] 10g of starch-biphenylyl chloride-aniline cross-linked copolymer, 10g of polyurethane imide modified starch, 12g of octenyl succinic anhydride modified starch and 15g of hydroxypropyl modified starch were placed in a 45°C oven for drying, crushed and mixed through an 80-mesh sieve to obtain a modified starch sample.

[0131] Example 5 Preparation of modified starch

[0132] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0133] 0.525 g of mung bean starch was irradiated under a 60Co-γ-ray irradiation source for 3 h, and then a 0.5% nitric acid solution was added and stirred to mix thoroughly. Then, 2.051 g of 3,3′,5,5′-biphenyltetrachloride and 1.101 g of aniline were added for cross-linking reaction. After ultrasonic treatment at a frequency of 32 kHz for 55 min, a 10% sodium hydroxide solution was slowly added dropwise to adjust the pH to 5, thereby obtaining a starch-biphenyl chloride-aniline cross-linked copolymer;

[0134] (2) preparing polyurethane imide modified starch;

[0135] First, 0.254 g of sodium hypochlorite was added to 1.625 g of mung bean starch to obtain oxidized starch, and then 2.525 g of oxidized starch, 0.045 g of polyurethane imide, 20 ml of glycerol, and 100 ml of acetone solution were mixed evenly, and reacted in a constant temperature water bath at 90 ° C for 2 h. After the reaction was completed, the temperature was lowered to 70 ° C and reacted in a constant temperature water bath for 0.6 h to obtain polyurethane imide modified starch;

[0136] (3) preparing octenyl succinic anhydride modified starch;

[0137] 1.368 g of mung bean starch and 0.784 g of octenyl succinic anhydride were mixed evenly, reacted in a constant temperature water bath at 55°C for 2 h, and then ultrasonically treated at a frequency of 32 kHz for 55 min, and then sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain octenyl succinic anhydride modified starch;

[0138] (4) preparing hydroxypropyl modified starch;

[0139] 1.025 g of a polyamine compound having a structure of formula (I) (m=6, n=8), 1.589 g of carboxymethyl chitosan, and 1.527 g of hydroxypropyl chitosan were added to a 5% hydrofluoric acid solution, stirred evenly, and then 8.282 g of mung bean starch was added, and the mixture was reacted in a constant temperature water bath at 45° C. for 2 h to obtain a hydroxypropyl modified starch;

[0140] (5) preparing modified starch;

[0141] 8.14 g of starch-biphenylyl chloride-aniline cross-linked copolymer, 7.05 g of polyurethane imide modified starch, 9.21 g of octenyl succinic anhydride modified starch and 6.25 g of hydroxypropyl modified starch were placed in a 45°C oven for drying, crushed and mixed through an 80-mesh sieve to obtain a modified starch sample.

[0142] Example 6 Preparation of modified starch

[0143] (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer;

[0144] After irradiating 1.6 g of potato starch under a 60Co-γ-ray irradiation source for 3 h, a 0.5% hydrochloric acid solution was added and stirred to be fully mixed, and then 2.532 g of 2,2′,4,4′-biphenyltetrachloride and 1.536 g of aniline were added for cross-linking reaction, and after ultrasonic treatment at a frequency of 25 kHz for 45 min, a 10% sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain a starch-biphenyl chloride-aniline cross-linked copolymer;

[0145] (2) preparing polyurethane imide modified starch;

[0146] First, 0.265 g of sodium sulfate was added to 1.562 g of potato starch to obtain oxidized starch, and then 3.254 g of oxidized starch, 0.0954 g of polyurethane imide, 20 ml of glycerol, and 100 ml of acetone solution were evenly mixed, and reacted in a constant temperature water bath at 95° C. for 2 h. After the reaction was completed, the temperature was lowered to 75° C. and reacted in a constant temperature water bath for 0.5 h to obtain polyurethane imide modified starch;

[0147] (3) preparing octenyl succinic anhydride modified starch;

[0148] 1.877 g of potato starch and 0.569 g of octenyl succinic anhydride were uniformly mixed, reacted in a constant temperature water bath at 60°C for 2.5 h, and then ultrasonically treated at a frequency of 30 kHz for 60 min, and then sodium hydroxide solution was slowly added dropwise to adjust the pH to 5 to obtain octenyl succinic anhydride modified starch;

[0149] (4) preparing hydroxypropyl modified starch;

[0150] 1.698 g of a polyamine compound having a structure of formula (III), 2.056 g of carboxymethyl chitosan, and 1.458 g of hydroxypropyl chitosan were added to a 5% acetic acid solution, stirred evenly, and then 10.424 g of potato starch was added, and the mixture was reacted in a constant temperature water bath at 48° C. for 1.8 h to obtain a hydroxypropyl modified starch;

[0151] (5) preparing modified starch;

[0152] 6.985 g of starch-biphenylyl chloride-aniline cross-linked copolymer, 6.874 g of polyurethane imide modified starch, 8.963 g of octenyl succinic anhydride modified starch and 10.54 g of hydroxypropyl modified starch were placed in a 50°C oven for drying, crushed and mixed through an 80-mesh sieve to obtain a modified starch sample.

[0153] Test Example 1 Storage Period Test

[0154] The modified starches prepared in Examples 1-6 were placed at room temperature (20° C.-30° C.) to test their storage periods. The test results are shown in Table 1.

[0155] Table 1

[0156]

[0157]

[0158] It can be seen from the data in Table 1 that the modified starch prepared by the present invention can be stored for 29-30 days at room temperature (20°C-30°C), and the storage period at 20°C, 25°C, and 30°C does not change much.

[0159] Test Example 2 Application of the modified starch prepared by the present invention in the preparation of wood adhesive

[0160] The modified starch prepared in Examples 1-6 was used as a wood adhesive in the production of multi-layer wood, and the bonding strength between the multi-layer wood was tested. The specific test process is as follows:

[0161] The modified starch prepared by the present invention is added to deionized water to prepare an emulsion, and an elm veneer with a thickness of 3 mm and a moisture content of 15% is selected, and the amount of glue is set to 318 g / m 2 According to the traditional multi-layer wood production process, three-layer and five-layer multi-layer composite elm boards were obtained through assembly, cold pressing and hot pressing processes. After the obtained multi-layer composite elm boards were stored for 24 hours, the gluing properties of the boards were tested according to the national standard GB9846-2004. The results are shown in Table 2.

[0162] Table 2

[0163] project Whether the glue is opened Bonding strength (normal, MPa) Bonding strength (Class II, MPa) Example 1 no 1.57 0.97 Example 2 no 1.62 0.88 Example 3 no 1.59 0.94 Example 4 no 1.60 0.95 Example 5 no 1.58 0.95 Example 6 no 1.59 0.96

[0164] It can be seen from the data in Table 2 that the use of the modified starch of the present invention as a wood adhesive meets the relevant requirements of the national standard GB9846-2004.

[0165] In summary, the modified starch prepared by the present invention has good stability and bonding performance, is not easy to agglomerate and delaminate, has a longer storage period, does not have carbonization problems during use, has improved bonding ability and gluing efficiency, and can greatly improve the service life of wood.

[0166] The present invention discloses a modified starch and a preparation method and application thereof. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The product of the present invention has been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the product described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

Claims

1. A method for preparing modified starch, characterized in that: The following steps are involved: (1) preparing starch-biphenylyl chloride-aniline cross-linked copolymer; After irradiating the starch under a 60Co-γ-ray irradiation source, a strong acid solution is added and stirred to fully mix, and then diphenyl chloride and aniline are added for cross-linking reaction, and after ultrasonic treatment, a sodium hydroxide solution is slowly added dropwise to adjust the pH to 4-6 to obtain a starch-diphenyl chloride-aniline cross-linked copolymer; (2) preparing polyurethane imide modified starch; First, an oxidant is added to starch to obtain oxidized starch, and then the oxidized starch, polyurethane imide, glycerol and acetone solution are uniformly mixed, and then reacted in a constant temperature water bath of 85°C-95°C for 1.5h-2.5h. After the reaction is completed, the temperature is lowered to a constant temperature water bath of 60°C-80°C for 0.5h-1h to obtain polyurethane imide modified starch; (3) preparing octenyl succinic anhydride modified starch; After the starch and octenyl succinic anhydride are uniformly mixed, the mixture is reacted in a constant temperature water bath at 55°C-60°C for 1.5h-2.5h, and after ultrasonic treatment, a sodium hydroxide solution is slowly added dropwise to adjust the pH to 4-6 to obtain octenyl succinic anhydride modified starch; (4) preparing hydroxypropyl modified starch; Add polyamine compound, carboxymethyl chitosan and hydroxypropyl chitosan in a mass ratio of (0.5-1.5): (1.3-2.1): (1.4-1.9) to a weak acid solution, stir evenly, add twice the weight of starch, and react in a constant temperature water bath at 40°C-50°C for 1h-2h to obtain hydroxypropyl modified starch; (5) preparing modified starch; The obtained starch-biphenyl chloride-aniline cross-linked copolymer, polyurethane imide modified starch, octenyl succinic anhydride modified starch and hydroxypropyl modified starch were placed in an oven at 40°C-50°C in a mass ratio of (4-10):(5-10):(7-15):(5-15), and then crushed, sieved and mixed to obtain a modified starch sample.

2. The method for preparing modified starch according to claim 1, characterized in that: In steps (1) to (4), the starch is selected from one of corn starch, mung bean starch, sweet potato starch, cassava starch, sweet potato starch, water chestnut starch, wheat starch, potato starch, and lotus root starch.

3. The method for preparing a modified starch according to claim 1, characterized in that: In step (1) and step (3), the frequency of the ultrasonic treatment is 25kHz-35kHz, and the time is 40min-100min.

4. The method for preparing modified starch according to claim 1, characterized in that: In step (1), the mass ratio of starch, benzyl chloride and aniline is (0.4-1.6):(1.7-2.6):(1.0-2.5).

5. The method for preparing modified starch according to claim 1, characterized in that: In step (1), the biphenyl chloride is selected from one of 2,2′,4,4′-biphenyl tetrachloride, 2,2′,5,5′-biphenyl tetrachloride, 3,3′,5,5′-biphenyl tetrachloride, 2,3′,4,5′,6,-biphenyl pentachloride or 2,2′,4,4′,6,6′-biphenyl hexachloride; The structural formula of the 2,2′,4,4′-biphenyltetraacyl chloride is: The structural formula of the 2,2′,5,5′-biphenyltetraacyl chloride is: The structural formula of the 3,3′,5,5′-biphenyltetraacyl chloride is: The structural formula of the 2,3′,4,5′,6-biphenylpentachloride is: The structural formula of the 2,2′,4,4′,6,6′-biphenylhexachloride is:

6. The method for preparing modified starch according to claim 1, characterized in that: In step (1), the strong acid solution is selected from one of sulfuric acid solution, nitric acid solution and hydrochloric acid solution; in step (4), the weak acid solution is selected from one of acetic acid and hydrofluoric acid.

7. The method for preparing modified starch according to claim 1, characterized in that: In step (2), the oxidant is selected from one of sodium hypochlorite, hydrogen peroxide, sodium sulfate, ammonium persulfate, and potassium permanganate.

8. The method for preparing modified starch according to claim 1, characterized in that: In step (4), the polyamine compound has a structure of formula (I), formula (II) or formula (III): Where m = 2-10, n = 2-10; Where R = C 11 H 23 , n = 9; Among them, n=16.

9. The modified starch prepared by the method for preparing modified starch according to claim 1.