Wear-resistant polyolefin pipeline lining material and preparation method of pipeline

By adding silicone masterbatches and polysiloxane to polyolefin pipeline materials, combined with the extrusion granulation process, the lack of wear resistance and processing properties of HDPE and polyolefin elastomers is solved, and the material resistance is significantly improved Abrasive properties and toughness extend service life and reduce processing costs.

CN119060445APending Publication Date: 2024-12-03SHANDONG WENYUAN BUILDING MATERIALS TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411315213.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing HDPE pipes have poor wear resistance and heat stability in agricultural irrigation, mine fine particle solid transport and sewage transport, and there are shortcomings in processing and performance of ultra-high molecular weight polyethylene and polyolefin elastomers, which are difficult to Improve its wear resistance through common methods.

Method used

Using silicone masterbatch as a modified filler, the wear resistance of polyolefin pipe lining materials is improved through the combination with polyolefin resin and the extrusion granulation process, and the polysiloxane content is increased to improve the toughness and flowability of the material. , reduce processing costs.

Benefits of technology

It significantly improves the abrasion resistance of polyolefin pipe materials, extends service life, reduces processing costs, and does not require additional auxiliary equipment or special treatments. It has simple process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060445A_ABST
    Figure CN119060445A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to a wear-resistant polyolefin pipeline lining material and a preparation method of a pipeline. The wear-resistant polyolefin pipeline lining material comprises the following raw materials in parts by weight: 100 parts of polyolefin resin and 5-50 parts of silicone master batch, the polyolefin resin is one or a combination of HDPE (High-Density Polyethylene) and POE (Polyolefin Elastomer), or a combination of POE and UHMWPE (Ultra High Molecular Weight Polyethylene); the addition ratio of HDPE to POE is (0-100): (0-100); the ratio of the POE to the UHMWPE is (60-99): (1-40). According to the invention, a large amount of silicone master batch is creatively added to improve the wear resistance of the pipe material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a wear-resistant polyolefin pipeline lining material and a preparation method of the pipeline. Background Art

[0002] In the use of pipes, high-density polyethylene (HDPE) pipes have a special hollow wall structure, which reduces the specific gravity of the pipes, enhances the ring stiffness, and has a small equipment investment, so they are widely used. However, HDPE as a pipe also has some shortcomings, such as low mechanical properties, poor wear resistance and heat resistance stability; especially in some occasions such as agricultural irrigation and transportation, HDPE pipes for transporting fine particles in mines, and sewage pipes that are often eroded by water and sand, which require HDPE to have good friction properties. Modification is carried out to meet the requirements for its wear resistance.

[0003] Ultra-high molecular weight polyethylene (UHMWPE) has a very high relative molecular mass, which can even reach more than 1.5 million. It is a linear unbranched polyethylene material. Although the molecular structure of ultra-high relative molecular weight polyethylene is basically the same as that of ordinary polyethylene, its unique structure gives it excellent properties such as low friction coefficient, wear resistance, impact resistance, and self-lubrication. Although ultra-high molecular weight polyethylene has many excellent properties, it also has many shortcomings. For example, due to its high molecular weight, its processable solution concentration is low and its viscosity is high. It cannot usually be prepared by general thermoplastic processing methods, and it has the disadvantages of low toughness, low mechanical strength, poor high temperature resistance, and poor creep resistance. In order to make up for these shortcomings, its performance can be optimized through reasonable modification.

[0004] Polyolefin elastomer (POE) is a random copolymer elastomer formed by copolymerization of ethylene and octene. It is a new homogeneous polyolefin polymer with unique molecular and rheological properties. The molecular chain is saturated, contains relatively few tertiary carbon atoms, has a narrow relative molecular weight distribution and short chain distribution, has good heat aging resistance and UV resistance, physical and mechanical properties, elasticity, strength, and elongation. It has the high elasticity and toughness of rubber at room temperature, has the characteristics of low density, large bending, high low-temperature impact resistance, easy processing, reusability, low price, etc., and does not require any plasticizer during molding. Therefore, it is widely used in photovoltaic cells, automotive parts, aerospace and other fields, greatly impacting traditional rubber, plastic and other materials. During processing, POE has a certain fluidity after the temperature reaches the melting point, can easily fill the mold, and it shrinks little during the cooling process, is not easy to deform, and saves a lot of energy for the operator. However, the wear resistance of POE material is relatively poor, which limits its application in some high wear occasions. At present, the methods for improving the wear resistance of POE mainly include adding wear-resistant agents, surface modification, etc., but the effect is limited.

[0005] It is necessary to develop new, convenient and simple methods to prepare low-cost, easy-to-make composite materials with high wear resistance to meet the actual needs of various fields. At present, the modification methods of common pipeline materials are generally complicated. Usually, a variety of fillers and resin matrices are required for extrusion granulation, and then the mixed particles are used for production. This process improves the performance of pipeline materials to meet the market demand for pipeline material performance. Some pipe materials have strict requirements on processing conditions and need to purchase equipment that meets production conditions, which increases the production cost of enterprises. Summary of the invention

[0006] The invention provides a wear-resistant polyolefin pipeline lining material, so as to achieve the purpose of improving the wear resistance of the pipe material, increasing the toughness of the plastic, extending the service life and enhancing the safety.

[0007] At the same time, the present invention also provides a method for preparing a pipeline of the wear-resistant polyolefin pipeline lining material.

[0008] A wear-resistant polyolefin pipe lining material, characterized by comprising the following raw materials in parts by weight:

[0009] 100 parts of polyolefin resin, 5-50 parts of silicone masterbatch;

[0010] The polyolefin resin is one of HDPE and POE or a combination of two of them, or a combination of POE and UHMWPE; the addition ratio is: HDPE:POE=0-100:0-100; POE:UHMWPE=60-99:1-40.

[0011] Preferably, the polysiloxane content of the silicone masterbatch is 50%, and the molecular weight of the silicone resin is 1.1-1.2 million.

[0012] The method for preparing the pipe of the wear-resistant polyolefin pipe lining material comprises the following steps:

[0013] Step 1: Mix the polyolefin resin and silicone masterbatch evenly at room temperature;

[0014] Step 2: The above mixture is extruded into granules using a single screw or twin screw extruder, and the process parameters are as follows:

[0015] Main machine temperature: Zone 1: 80-130℃, Zone 2: 100-150℃, Zone 3: 130-200℃, Zone 4: 130-200℃, Zone 5: 130-200℃, Zone 6: 130-200℃, Machine head temperature: 130-200℃;

[0016] Speed: 10-100 rpm;

[0017] Step 3: Cooling and shaping, cutting and granulating to obtain polyolefin wear-resistant lining material;

[0018] Step 4: Use a single screw or twin screw to extrude the polyolefin wear-resistant lining material and high-density polyethylene into a pipe through a co-extrusion process; the high-density polyethylene is the outer layer of the wear-resistant composite pipe, and the inner layer is made of polyolefin wear-resistant lining material to reduce pipe wear; the process parameters are as follows:

[0019] Main machine temperature: Zone 1: 80-130℃, Zone 2: 100-150℃, Zone 3: 130-200℃, Zone 4: 130-200℃, Zone 5: 130-200℃, Zone 6: 130-200℃, Machine head temperature: 130-200℃;

[0020] Speed: 10-100 rpm;

[0021] Step 5: The pipe cools and takes shape.

[0022] Beneficial effects of the present invention:

[0023] In the prior art, the amount of silicone masterbatch added is small, and it is only used as an auxiliary filler to improve the processing performance of the material. However, in the present invention, a large amount of silicone masterbatch is added to improve the wear resistance of the pipe material:

[0024] From the perspective of production equipment and process, no auxiliary equipment needs to be added during the production process, and the raw materials do not need to be specially treated. Production can be carried out after they are evenly mixed. The process is simple, the cost is low, and it has the advantages of good processability, high toughness, and good abrasion resistance. The different melting points of the raw materials can appropriately reduce the polymer processing temperature and reduce the processing cost of the polymer material. Compared with unmodified polyolefin materials, the raw materials in the present invention have better processing performance and improved abrasion resistance.

[0025] In the present invention, silicone masterbatch is used as the only modified filler, and its main component is polysiloxane, which can provide internal and external lubrication for plastic products and reduce the phenomenon of melt fracture during the processing and molding of products. It can significantly improve the fluidity of plastic melt, improve the processing performance, anti-friction and wear resistance of polyolefin; polysiloxane increases the cross-linking density of polyolefin, and can also effectively improve the toughness of plastic, making it not easy to break under impact, bending, friction and other conditions, thereby improving the service life and safety of plastic products.

[0026] In the present invention, the silicone masterbatch is selected as a modifier by scientific proportioning, and the wear-resistant material is extruded after mixing. Compared with unmodified HDPE, the wear resistance of modified HDPE is improved by 20-40%, and the wear resistance of modified POE is improved by 60-80% compared with unmodified POE. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1It is a schematic diagram of the structure of the wear-resistant polyolefin pipeline of the present invention;

[0028] In the figure: 1. High-density polyethylene; 2. Polyolefin wear-resistant lining material; DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further explained below through specific implementation methods.

[0030] A wear-resistant polyolefin pipe lining material comprises the following raw materials in parts by weight: 100 parts of polyolefin resin and 5-50 parts of silicone masterbatch; the polyolefin resin is one or a combination of HDPE and POE, or a combination of POE and UHMWPE; the adding ratio is: HDPE:POE=0-100:0-100; POE:UHMWPE=60-99:1-40.

[0031] The polysiloxane content of the silicone masterbatch is 50%, and the molecular weight of the silicone resin is 1.1-1.2 million.

[0032] POE characteristic parameters: specific gravity: 0.9080g / cm 3 , melt index: 1.0g / 10min, Mooney viscosity: 20MU, elongation at break: 750%, tensile strength at break: 27.9MPa;

[0033] HDPE characteristic parameters: specific gravity: 0.9495g / cm 3 , melt index: 0.2g / 10min, elongation at break: 771%, tensile yield strength: 22.3MPa;

[0034] UHMPE performance parameters: specific gravity: 0.9300g / cm 3 , melt index: 0.1g / 10min, elongation at break: 50%, tensile yield strength: 20MPa.

[0035] The raw material components added in each embodiment are as follows in Table 1:

[0036]

[0037] Example 9

[0038] The method for preparing the pipe of the wear-resistant polyolefin pipe lining material comprises the following steps:

[0039] Step 1: Mix the polyolefin resin and silicone masterbatch evenly at room temperature;

[0040] Step 2: Extruding the above mixture into a pipe using a single screw or twin screw extruder, the process parameters are as follows:

[0041] Main machine temperature: Zone 1: 80-130℃, Zone 2: 100-150℃, Zone 3: 130-200℃, Zone 4: 130-200℃, Zone 5: 130-200℃, Zone 6: 130-200℃, Machine head temperature: 130-200℃;

[0042] Speed: 10-100 rpm;

[0043] Step 3: Cooling and shaping, cutting and granulating to obtain polyolefin wear-resistant lining material;

[0044] Step 4: Use a single screw or twin screw to extrude the polyolefin wear-resistant lining material and high-density polyethylene into a pipe through a co-extrusion process; the high-density polyethylene 1 is the outer layer of the wear-resistant composite pipe, and the inner layer is made of the polyolefin wear-resistant lining material 2 to reduce the wear of the pipe; the process parameters are as follows:

[0045] Main machine temperature: Zone 1: 80-130℃, Zone 2: 100-150℃, Zone 3: 130-200℃, Zone 4: 130-200℃, Zone 5: 130-200℃, Zone 6: 130-200℃, Machine head temperature: 130-200℃;

[0046] Speed: 10-100 rpm;

[0047] Step 5: Pipe cooling and shaping

[0048] When the raw materials of Example 1 are produced, the following steps are followed:

[0049] Step 1: Mix the polyolefin resin and silicone masterbatch evenly at room temperature;

[0050] Step 2: Extruding the above mixture into a pipe using a single screw or twin screw extruder, the process parameters are as follows:

[0051] Mainframe temperature: Zone 1: 90℃, Zone 2: 150℃, Zone 3: 190℃, Zone 4: 190℃, Zone 5: 190℃, Zone 6: 190℃, Head temperature: 190℃;

[0052] Speed: 30 rpm;

[0053] Step 3: Cooling and shaping, cutting and granulating to obtain polyolefin wear-resistant material;

[0054] Step 4: Use a single screw or a twin screw to extrude the polyolefin wear-resistant material in step 3 and the high-density polyethylene into a pipe through a co-extrusion process; the process parameters are as follows:

[0055] Mainframe temperature: Zone 1: 90℃, Zone 2: 150℃, Zone 3: 190℃, Zone 4: 190℃, Zone 5: 190℃, Zone 6: 190℃, Head temperature: 190℃;

[0056] Speed: 30 rpm

[0057] Step 5: Pipe cooling and shaping

[0058] The other embodiments are manufactured according to the preparation method.

[0059] The wear resistance of the material was tested in accordance with DB / T 2450-2018 "General Technical Specifications for Polyolefin Composite Wear-Resistant Pipes". The sample size was 80×25×7.2mm and the abrasion was carried out in the mortar at a speed of 669±30r / min. The wear rate calculation method is as follows:

[0060]

[0061] m1 is the mass before wear; m2 is the mass after wear. The wear rates of the pipes produced by the raw materials of Example 1 to Example 8 are shown in Table 2:

[0062] Group Wear rate Unmodified HDPE 0.011 Unmodified POE 0.053 Example 1 0.019 Example 2 0.006 Example 3 0.011 Example 4 0.013 Example 5 0.021 Example 6 0.023 Example 7 0.008 Example 8 0.003

[0063] Pure POE and pure HDPE were modified using silicone masterbatch, and the experimental results showed that the wear of both materials was significantly reduced, which proves that the use of silicone masterbatch as a modifier to modify polyolefins can improve the wear resistance of polyolefin materials. For HDPE / POE / silicone composites, increasing the POE content can improve the processability of the composites, but at the same time it will reduce its wear resistance. Although adding UHMWPE as a reinforcing phase to the composite can improve the wear resistance of POE / UHMWPE / silicone composites, it will also cause the fluidity of the composite to decrease, thereby increasing the difficulty of processing. Increasing the content of silicone masterbatch will improve the wear resistance of the material, but too high a content will have a negative impact on the performance.

Claims

1. A wear-resistant polyolefin pipe lining material, characterized in that: The composition comprises the following raw materials in parts by weight: 100 parts of polyolefin resin, 5-50 parts of silicone masterbatch; The polyolefin resin is one of HDPE and POE or a combination of two of them, or a combination of POE and UHMWPE; the addition ratio is: HDPE:POE=0-100:0-100; POE:UHMWPE=60-99:1-40.

2. The wear-resistant polyolefin pipe material according to claim 1, characterized in that: The polysiloxane content of the silicone masterbatch is 50%, and the molecular weight of the silicone resin is 1.1-1.2 million.

3. A method for preparing a pipe of the wear-resistant polyolefin pipe lining material according to claim 1, comprising the following steps: Step 1: Mix the polyolefin resin and silicone masterbatch evenly at room temperature; Step 2: The above mixture is extruded into granules using a single screw or twin screw extruder, and the process parameters are as follows: Main machine temperature: Zone 1: 80-130℃, Zone 2: 100-150℃, Zone 3: 130-200℃, Zone 4: 130-200℃, Zone 5: 130-200℃, Zone 6: 130-200℃, Machine head temperature: 130-200℃; Speed: 10-100 rpm; Step 3: Cooling and shaping, cutting and granulating to obtain polyolefin wear-resistant lining material; Step 4: Use a single screw or twin screw to extrude the polyolefin wear-resistant lining material and high-density polyethylene into a pipe through a co-extrusion process; the high-density polyethylene is the outer layer of the wear-resistant composite pipe, and the inner layer is made of polyolefin wear-resistant lining material to reduce pipe wear; the process parameters are as follows: Main machine temperature: Zone 1: 80-130℃, Zone 2: 100-150℃, Zone 3: 130-200℃, Zone 4: 130-200℃, Zone 5: 130-200℃, Zone 6: 130-200℃, Machine head temperature: 130-200℃; Speed: 10-100 rpm; Step 5: The pipe cools and takes shape.

Citation Information

Cited By

  • Composite ore pulp conveying pipeline with POE (Polyolefin Elastomer) as wear-resistant layer and preparation method of composite ore pulp conveying pipeline

    CN120557451A