Polypropylene composite material as well as preparation method and application thereof
The polypropylene composite material with maleic anhydride and glycidyl methacrylate grafts improves impact performance and maintains mechanical properties, addressing the limitations of existing composites.
Patent Information
- Application Number
- CN202310624091.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-30
AI Technical Summary
Existing polypropylene and carbon fiber composite materials fail to significantly improve impact performance while maintaining mechanical properties such as high tensile strength and modulus.
A polypropylene composite material is prepared using maleic anhydride and glycidyl methacrylate grafts as compatibilizers, combined with chopped carbon fibers, β-nucleating agents, and antioxidants, enhancing interfacial compatibility and toughness through a specific preparation method involving twin-screw extrusion.
The composite material achieves high tensile strength, high tensile modulus, and high impact strength, making it suitable for automotive applications.
Smart Images

Figure BDA0004256371620000021 
Figure BDA0004256371620000041 
Figure BDA0004256371620000051
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically to a polypropylene composite material and a preparation method and application thereof. Background Art
[0002] Polypropylene material has the characteristics of low density, chemical resistance and excellent cost performance, and has been widely used in automotive interior and exterior parts.
[0003] Carbon fiber is a new type of fiber material with high strength and high modulus. The material properties are mainly composed of carbon elements. It has the advantages of high temperature resistance, friction resistance, water resistance, corrosion resistance and low density. It is added to polymers as a reinforcing material to obtain polymer composite materials, which can greatly improve the comprehensive mechanical properties of polymers.
[0004] Polypropylene is a thermoplastic resin with excellent performance. Carbon fiber reinforced polypropylene composite materials can play a unique advantage in meeting the demand for lightweight automobiles. Short-cut carbon fiber reinforced materials with high tensile strength, high tensile modulus and high impact strength are still technical issues that need to be urgently solved in this field.
[0005] The existing technology improves the compatibility of polypropylene resin and carbon fiber by adding maleic anhydride grafted polypropylene, maleic anhydride grafted POE, ethylene-butyl acrylate grafted maleic anhydride, ethylene-butyl acrylate grafted glycidyl methacrylate, epoxy resin, etc. to the composite material of polypropylene and carbon fiber. It only solves the rigidity problem of continuous carbon fiber reinforced materials, and there is still no solution to the impact strength of chopped carbon fiber reinforced polypropylene materials. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing composite materials of polypropylene and carbon fiber, which result in the inability to significantly improve the impact performance of the material while maintaining the mechanical properties of the material, and to provide a polypropylene composite material that can significantly improve the impact performance of the material while maintaining the mechanical properties of the material, and can enable the material to have high tensile strength, high tensile modulus and high impact strength at the same time.
[0007] Another object of the present invention is to provide a method for preparing a polypropylene composite material.
[0008] Another object of the present invention is to provide an application of a polypropylene composite material in the preparation of automobile interiors or automobile exteriors.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] A polypropylene composite material, comprising the following components by weight:
[0011]
[0012]
[0013] The polar grafted material A is a maleic anhydride grafted material, and the mass grafting rate of maleic anhydride is 0.7-1.3%. The mass grafting rate of maleic anhydride is tested by acid-base titration under the conditions of titration with KOH-ethanol solution at 75°C.
[0014] The polar graft B is a glycidyl methacrylate (GMA) graft, and the mass graft rate of glycidyl methacrylate is 0.6-0.8%. The mass graft rate of glycidyl methacrylate is tested by FTIR, the test conditions are potassium bromide tableting, and the test epoxy characteristic peak area is calculated.
[0015] The present invention uses maleic anhydride grafts and GMA grafts as compatibilizers for glass fiber reinforced polypropylene, while maintaining the mechanical strength performance at room temperature, and can improve the impact performance of the material. This is because the polar structures in maleic anhydride and GMA effectively coat the carbon fiber surface to improve the material interface strength, while the epoxy group and the carboxyl group react to form an interpenetrating network to maintain the high rigidity and high toughness of the material.
[0016] Preferably, the weight ratio of the polar graft B to the polar graft A is 0.6-1.
[0017] Preferably, the polar grafted material A is one or more of maleic anhydride grafted polypropylene and maleic anhydride grafted polyethylene.
[0018] More preferably, the polar grafted substance A is maleic anhydride grafted polypropylene.
[0019] Preferably, the polar grafted material B is one or more of glycidyl methacrylate grafted polyolefin elastomer and glycidyl methacrylate grafted polypropylene.
[0020] More preferably, the polar grafted substance B is glycidyl methacrylate grafted polyolefin elastomer.
[0021] Optionally, the average length of the chopped carbon fibers is 2.5-11 mm.
[0022] Preferably, the average length of the chopped carbon fibers is 3.0-9.0 mm.
[0023] The average length of the chopped carbon fibers affects the ultimate tensile strength in the material.
[0024] β-nucleating agent is beneficial to the formation of β-crystal in polypropylene resin, so that the crystal size of polypropylene is smaller and the structure is more uniform, thereby improving the rigidity and toughness balance of the material.
[0025] Preferably, the β-nucleating agent is one or more of aryl dimethyl amide, calcium pimelate or calcium suberate.
[0026] More preferably, the β-nucleating agent is aryl dimethyl amide.
[0027] Optionally, the melt mass flow rate of the polypropylene resin is 10 to 150 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
[0028] Preferably, the melt mass flow rate of the polypropylene resin is 30 to 100 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
[0029] Optionally, the polypropylene resin is homopolypropylene and / or copolymer polypropylene.
[0030] Preferably, the polypropylene resin is homopolypropylene.
[0031] Preferably, the antioxidant is one or more of a hindered phenol antioxidant, a phosphite antioxidant or a thioester antioxidant.
[0032] Optionally, the hindered phenol antioxidant is one or more of antioxidants 1010, 1976 or 3114.
[0033] Optionally, the phosphite antioxidant is one or more of antioxidants 168, 626 or PEP-36.
[0034] Optionally, the weight ratio of the hindered phenol antioxidant to the phosphite antioxidant is 1:1.
[0035] Antioxidants can improve the antioxidant effect of polypropylene composites.
[0036] The invention also protects a preparation method of a polypropylene composite material, comprising the following steps: mixing the components, melting and extruding through an extruder, granulating, and drying to obtain the polypropylene composite material.
[0037] Preferably, the preparation method of the polypropylene composite material comprises the following steps: mixing the components except the chopped carbon fiber, adding the components into a twin-screw extruder from the main feed port of the extruder, adding the chopped carbon fiber into the extruder from the side feed port of the extruder, and obtaining the polypropylene composite material after melt extrusion, granulation and drying.
[0038] The extruder may be a twin-screw extruder.
[0039] The preparation method of the polypropylene composite material of the present invention can be prepared by the following steps:
[0040] S1. The polypropylene resin, polar graft A, polar graft B, antioxidant and nucleating agent are weighed in parts by mass and added to a high mixer for mixing, and then added to a twin-screw extruder with an aspect ratio of 40:1 for melt mixing and dispersion. After plasticization by the twin-screw extruder, the twin-screw extruder is set at a temperature of 180°C to 200°C and a screw speed of 400 to 450 rpm;
[0041] S2. Add the chopped carbon fiber from the side feed port of the twin-screw extruder, set the temperature of the side feed port screw barrel to 180°C to 200°C, and obtain a polypropylene composite material after traction, cooling, pelletizing and drying.
[0042] The polypropylene composite material prepared by the present invention has high tensile strength, high tensile modulus and high impact strength, and can be widely used in the preparation of plastic products. The present invention particularly protects the use of the polypropylene composite material in the preparation of automobile parts, especially automobile interiors and / or automobile exteriors.
[0043] The automobile interior can be one or more of the dashboard frame, central channel or door panel bracket.
[0044] The automobile exterior decoration may be one or more of a bumper support, a cross-cable beam (CCB) or a bottom guard plate.
[0045] An automobile component is made by injection molding any one of the above-mentioned polypropylene composite materials.
[0046] Preferably, the automotive component is an automotive interior / exterior trim.
[0047] The automobile interior is a door substrate, a door lock bracket or a bumper bracket, etc.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] The polypropylene composite material of the present invention comprises polypropylene resin, chopped carbon fibers, polar grafts A, polar grafts B, β-nucleating agents, and antioxidants. The synergistic effect of adding specific polar grafts A and polar grafts B effectively improves the interfacial compatibility of polypropylene and carbon fibers in the polypropylene composite material, and can significantly improve the impact performance of the material while maintaining the mechanical properties of the material, so that the material can have high tensile strength, high tensile modulus, and high impact strength at the same time.
[0050] The polypropylene composite material of the present invention has a tensile strength of ≥108MPa, a tensile modulus of ≥10300MPa, and an impact strength of ≥9.6kJ / m 2 . DETAILED DESCRIPTION
[0051] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0052] The raw materials used in the embodiments and comparative examples of the present invention are shown in Table 1 below.
[0053] Table 1
[0054]
[0055]
[0056] The preparation method of the polar grafted material B3 is as follows: 1.5% by mass of GMA, 0.2% by mass of styrene, 98.3% by mass of POE 7467 and an initiator are uniformly mixed, added into a twin-screw extruder for extrusion, pelletized, dried and set aside, and the extrusion temperature is 160°C.
[0057] The preparation method of the polar grafted material B4 is as follows: 0.7% by mass of GMA, 0.2% by mass of styrene, 99.1% by mass of POE 7467 and an initiator are uniformly mixed, added into a twin-screw extruder for extrusion, pelletized, dried and set aside, and the extrusion temperature is 160°C.
[0058] The preparation method of the polar grafted material B5 is as follows: 0.8% by mass of GMA, 0.2% by mass of styrene, 99% by mass of POE7467 and an initiator are uniformly mixed, added into a twin-screw extruder for extrusion, pelletized, dried and set aside, and the extrusion temperature is 160°C.
[0059] Examples 1 to 21
[0060] A polypropylene composite material is prepared from the following components by weight: polypropylene resin; short-cut carbon fiber; polar graft A; polar graft B; beta nucleating agent; and antioxidant.
[0061] The specific content of each component is shown in Table 2 below.
[0062] Table 2 Composition of polypropylene composite materials in various embodiments (by weight)
[0063] Components 1 2 3 4 5 Polypropylene resin 1 62.3 80 50.3 62.3 62.3 Chopped carbon fiber 1 30 20 40 30 30 Polar grafted compound A1 4 3 5 4.5 3.6 Polar grafted compound B1 3.2 2.4 4 2.7 3.6 β-nucleating agent 1 0.1 0.1 0.1 0.1 0.1 Antioxidants 0.4 0.4 0.4 0.4 0.4
[0064] Table 2
[0065]
[0066]
[0067] Table 2
[0068] Components 17 18 19 20 21 Polypropylene resin 1 62.3 62.3 62.3 62.3 62.3 Chopped carbon fiber 1 30 30 30 30 30 Polar grafted compound A1 4 4 4 4 Polar grafted compound A6 4 Polar grafted compound B1 3.2 3.2 Polar grafted compound B2 3.2 Polar grafted compound B5 3.2 Polar grafted compound B6 3.2 β-nucleating agent 1 0.1 0.1 0.1 0.1 β-nucleating agent 2 0.1 Antioxidants 0.4 0.4 0.4 0.4 0.4
[0069] The preparation method of the polypropylene composite material comprises the following steps:
[0070] S1. The polypropylene resin, polar graft A, polar graft B, antioxidant and nucleating agent were weighed in parts by mass and added to a high mixer for 5 minutes, added to a twin-screw extruder with an aspect ratio of 40:1 for melt mixing and dispersion, and after plasticization by a twin-screw extruder, the screw speed was 450 rpm;
[0071] S2. The chopped carbon fiber is added from the side feed port of the twin-screw extruder, the temperature of the side feed port screw is set to 180 ° C, and after traction, cooling, pelletizing and drying, a polypropylene composite material is obtained;
[0072] The processing temperatures from the feed port to the die are: 100℃, 180℃, 180℃, 200℃, 200℃, 200℃, 180℃, 200℃, 200℃.
[0073] Comparative Examples 1 to 12
[0074] A polypropylene composite material comprises the following components by weight: polypropylene resin; short-cut carbon fiber; polar graft A; polar graft B; beta nucleating agent; and antioxidant.
[0075] The specific content of each component is shown in Table 3 below.
[0076] Table 3 Composition of polypropylene composite materials of each comparative example (by weight)
[0077] Components 1 2 3 4 5 6 7 8 9 10 11 12 Polypropylene resin 1 69.5 62.3 62.3 62.3 62.3 62.3 62.3 62.3 62.3 62.3 62.3 62.3 Chopped carbon fiber 1 30 30 30 30 30 30 30 30 30 30 30 30 Polar grafted compound A1 0 0 7 7.2 4 4 4 4 4 4 Polar grafted compound A3 4 Polar grafted compound A4 4 Polar grafted compound B1 0 7.2 3.2 0 6 3.2 3.2 3.2 3.2 3.2 Polar grafted compound B3 3.2 Polar grafted compound B4 3.2 β-nucleating agent 1 0.1 0.1 0.1 0.1 0.1 0.1 0.1 0.1 0.1 0 0.4 α Nucleating Agent 0.1 Antioxidants 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4
[0078] The preparation method of the polypropylene composite material is the same as that in the embodiment, and will not be described again here.
[0079] Results
[0080] The polypropylene composite materials of each embodiment and comparative example were tested according to the following method:
[0081] (1) Tensile strength: According to ISO 527-2016 method, tensile speed 10 mm / min.
[0082] (2) Tensile modulus: according to ISO 527-2016 method, tensile speed 1 mm / min.
[0083] (3) Impact performance: According to ISO 179-2016 method, 4 mm thick specimen, notch type is type A, pendulum impact capacity is 4.5J.
[0084] The specific test results of the polypropylene composite materials of each embodiment are described in Table 4 below:
[0085] Table 4
[0086] Example Tensile strength / MPa Tensile modulus / MPa <![CDATA[Impact strength / kJ / m 2 > 1# 122 13500 12 2# 108 10500 10 3# 131 17000 10 4# 119 12000 11 5# 120 12800 11 6# 120 12700 11 7# 118 12500 9.6 8# 110 10400 11 9# 115 11600 11 10# 108 11800 12 11# 116 12900 12 12# 112 12300 12 13# 110 10300 10 14# 111 11600 10 15# 118 12800 11 16# 118 12700 11 17# 110 12000 10 18# 118 12700 11 19# 117 12600 11 20# 116 12400 9.8 21# 119 12700 10
[0087] The specific test results of the polypropylene composite materials of each comparative example are described in Table 5 below: Table 5
[0088]
[0089]
[0090] From the above data, it can be seen that the polypropylene composite material of the present invention effectively improves the interfacial compatibility of polypropylene and carbon fiber in the polypropylene composite material by adding the synergistic effect of specific polar grafts A and polar grafts B, and can significantly improve the impact resistance of the material while maintaining the mechanical properties of the material, so that the material can have high tensile strength, high tensile modulus and high impact strength at the same time. The polypropylene composite material of the present invention has a tensile strength of ≥108MPa, a tensile modulus of ≥10300MPa, and an impact strength of ≥9.6kJ / m 2 .
[0091] It can be seen from Comparative Example 1 that without adding polar graft A and polar graft B, the tensile strength and tensile modulus of the material are obviously too low.
[0092] It can be seen from Comparative Example 2 that without adding the polar graft A, the impact strength of the material is too low.
[0093] It can be seen from Comparative Example 3 that if the amount of polar grafted material A added is too much, the impact strength will not meet the requirements.
[0094] It can be seen from Comparative Example 4 that without adding the polar graft B, the impact strength of the material is not improved.
[0095] It can be seen from Comparative Example 5 that if the amount of polar graft B added is too much, the impact strength will not meet the requirements due to the high elastomer content in the graft.
[0096] It can be seen from Comparative Examples 6 and 7 that in polar graft A, too high or too low mass grafting rate of maleic anhydride will cause a decrease in the tensile strength of carbon fiber reinforced polypropylene. If the mass grafting rate of maleic anhydride is too low, it is difficult to ensure the interface bonding between polar graft A and short carbon fibers. If the mass grafting rate of maleic anhydride is too high, it is not conducive to bonding with the polypropylene resin matrix, nor is it conducive to the improvement of tensile strength.
[0097] It can be seen from Comparative Examples 8 and 9 that in the polar grafted material B, the mass grafting rate of glycidyl methacrylate is too high or too low, and the impact strength of the material is not improved.
[0098] It can be seen from Comparative Examples 10 and 11 that not adding β-nucleating agent or adding too much β-nucleating agent will lead to a decrease in impact strength.
[0099] It can be seen from Comparative Example 12 that the use of an α nucleating agent leads to an increase in the crystallinity of the material, but the α crystal form is not conducive to the impact strength of the material.
[0100] It can be seen from Examples 1, 4 and 5 that when the weight ratio of the polar graft B to the polar graft A is 0.6-1, it is more conducive to the formation of a good synergistic effect between the polar grafts, which is beneficial to the improvement of strength and impact.
[0101] It can be seen from Examples 1 and 6 to 10 that the melt mass flow rate of the polypropylene resin mainly affects the tensile strength performance of the material, and a suitable flow rate can obtain good tensile strength.
[0102] The polypropylene resin is a homopolymer polypropylene resin, which is more conducive to tensile strength.
[0103] It can be seen from Examples 1 and 11 to 14 that
[0104] The length of chopped carbon fiber mainly affects the tensile strength performance of the material, and the longer the length, the higher the tensile strength. However, too long a length will cause dispersion problems and reduce the tensile strength.
[0105] It can be seen from Example 1, Example 15 to Example 16, Comparative Example 6 and Comparative Example 7 that the mass grafting rate of the polar graft A will affect the tensile strength of the material, and a suitable grafting rate is an important guarantee for improving the interface performance.
[0106] It can be seen from Example 1 and Example 17 that the polar graft A is maleic anhydride grafted polypropylene, which is more beneficial to tensile strength.
[0107] It can be seen from Example 1 and Example 20 that among the polar grafts B, the polar graft B which is glycidyl methacrylate grafted polyolefin elastomer is more beneficial to impact strength.
[0108] It can be seen from Example 1 and Example 21 that when the nucleating agent is an aromatic dimethylamide β-nucleating agent, it is more conducive to improving the impact strength of the material.
[0109] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A polypropylene composite material, characterized in that: By weight, it includes the following components: Wherein, the polar grafted material A is a maleic anhydride grafted material, and the mass grafting rate of maleic anhydride is 0.7-1.3%; The polar grafted material B is a glycidyl methacrylate grafted material, and the mass grafting rate of glycidyl methacrylate is 0.6-0.8%.
2. The polypropylene composite material according to claim 1, characterized in that: The weight ratio of the polar graft B to the polar graft A is 0.6-1.
3. The polypropylene composite material according to claim 1, characterized in that: The polar grafted material A is one or more of maleic anhydride grafted polypropylene and maleic anhydride grafted polyethylene.
4. The polypropylene composite material according to claim 1, characterized in that: The polar grafted substance B is one or more of glycidyl methacrylate grafted polyolefin elastomer and glycidyl methacrylate grafted polypropylene.
5. The polypropylene composite material according to claim 1, characterized in that: The average length of the chopped carbon fibers is 2.5-11 mm.
6. The polypropylene composite material according to claim 1, characterized in that: The beta nucleating agent is one or more of aryl dimethyl amide, calcium pimelate or calcium suberate.
7. The polypropylene composite material according to claim 1, characterized in that: The melt mass flow rate of the polypropylene resin is 10 to 150 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
8. The polypropylene composite material according to claim 1, characterized in that: The antioxidant is one or more of a hindered phenol antioxidant, a phosphite antioxidant or a thioester antioxidant.
9. The method for preparing the polypropylene composite material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing the components except the short-cut carbon fibers, adding the components into a twin-screw extruder from a main feeding port of the extruder, adding the short-cut carbon fibers into the extruder from a side feeding port of the extruder, and obtaining the polypropylene composite material after melt extrusion, granulation and drying.
10. Use of the polypropylene composite material according to any one of claims 1 to 8 in the preparation of automobile interior or exterior materials.
Citation Information
Patent Citations
Polypropylene (PP) composite material and preparation method thereof
CN102329457A
Polypropylene / nylon composite material and preparation method thereof
CN114410001A
Modified glass fiber and preparation method and application thereof
CN114672070A
Polypropylene composite material as well as preparation method and application thereof
CN114773727A
Poly propylene resin composition for interior materials of automobile
KR1020120045951A