High-pressure-resistant and weather-aging-resistant ethylene propylene diene monomer material and preparation method thereof
By polymerizing the hexagonal boron nitride and alkenyl modification, combined with surface grafting of aromatic ketone voltage stabilizers, modified functional fillers were prepared, solving the breakdown of ethylene propylene rubber in high pressure and outdoor environments and aging problems, the materials have achieved high pressure and climate aging resistance.
Patent Information
- Application Number
- CN202411438998.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ethylene propylene ternary rubber is prone to breakdown and aging problems in high voltage and outdoor environments, resulting in insufficient high voltage resistance and aromatic ketone voltage stabilizers are easy to migrate, making it difficult to effectively play their role.
Modification function was prepared by polymerizing and coating the hexagonal boron nitride with dopamine hydrochloride, and alkenyl modification of vinyl trimethoxysilane and surface grafting of 4-propyleneoxy-2-hydroxybenzophenone. The filler is kneaded and vulcanized with components such as EPDM, silicone rubber, carbon black, paraffin oil, etc. to form a new EPDM rubber material that is resistant to high pressure and climate aging.
It significantly improves the high-pressure resistance and climate aging effect of the material, ensures that it is not broken down under high pressure, and shows good aging resistance in outdoor environments, and is suitable for insulator fields.
Smart Images

Figure BDA0005085854580000111 
Figure BDA0005085854580000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of EPDM rubber, and in particular relates to an EPDM rubber material which is resistant to high pressure and weathering and a preparation method thereof. Background Art
[0002] As a widely used device in the insulation system, insulators play a vital role in the fields of electrical and power engineering. Among them, the materials used in insulators mainly include organic polymers with excellent insulation properties such as EPDM rubber and silicone rubber. However, the existing EPDM rubber still has certain disadvantages that limit its use effect in insulators. This is because on the one hand, the high-voltage resistance of EPDM rubber is still insufficient, and it will face breakdown problems under high-voltage and ultra-high-voltage environments, which seriously restricts the scope of use. Based on this, many existing technologies will choose to add aromatic ketone voltage stabilizers to EPDM rubber to improve the breakdown strength, that is, high-voltage resistance. However, most of these aromatic ketone voltage stabilizers are small molecular compounds, which are very easy to migrate from EPDM rubber under the action of electric field and heat, resulting in uneven distribution or loss, and it is difficult to play the technical effect well. On the other hand, since insulators are mostly used in outdoor environments, they inevitably need to experience long-term exposure to the sun. Therefore, the thermal effect accumulates seriously, which undoubtedly aggravates the aging process, and then leads to rapid growth of electric trees. Ultimately, it also has a greater adverse effect on the high-voltage resistance. Summary of the invention
[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide a high-voltage and weather-resistant ethylene propylene diene monomer (EPDM) rubber material and a preparation method thereof. The present invention firstly polymerizes and coats hexagonal boron nitride with dopamine hydrochloride to form an organic polymer interface, then adds vinyl trimethoxy silane to complete the first alkenyl modification, then uses 4-propyleneoxy-2-hydroxybenzophenone as a voltage stabilizer, polymerizes through double bonds to achieve surface grafting of the voltage stabilizer, and finally further adds vinyl trimethoxy silane to complete the second alkenyl modification, thereby preparing a modified functional filler, which is mixed with conventional components such as ethylene propylene diene monomer (EPDM) rubber, silicone rubber, carbon black, paraffin oil, antioxidant, etc., and subjected to vulcanization operations to obtain a novel ethylene propylene diene monomer (EPDM) rubber material, which not only has excellent high-voltage resistance, but also has good weather-resistant effect, and is very suitable for application in the field of insulators.
[0004] The purpose of the present invention can be achieved by the following technical solutions:
[0005] The invention discloses an EPDM rubber material which is resistant to high pressure and weathering. The EPDM rubber material is prepared from EPDM rubber, silicone rubber, modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer.
[0006] As a preferred technical solution of the present invention, the mass ratio of the EPDM rubber, the silicone rubber, the modified functional filler, the carbon black, the paraffin oil, the antioxidant, the accelerator and the vulcanizer is 100:35-40:8-10:50-55:15:0.2:1-1.5:3.
[0007] As a preferred technical solution of the present invention, the modified functional filler is prepared by the following steps:
[0008] Step A: adding 1-1.5 parts by weight of dopamine hydrochloride and 2-2.5 parts by weight of hexagonal boron nitride to 120-140 parts by weight of Tris-HCl buffer, and then stirring ultrasonically at 30-40° C. for 10-12 hours in contact with air, filtering, taking the filter residue, washing it with deionized water, and finally vacuum drying it at 50-70° C. until constant weight, to obtain component A;
[0009] Step B: adding the component A, 0.5-1 parts by weight of vinyltrimethoxysilane and 1-2 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, stirring for 14-16 hours at 60-70° C. in the dark, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 50-70° C. until constant weight, to obtain component B;
[0010] Step C: adding 20-30 parts by weight of dimethyl sulfoxide, the component B, 1-1.5 parts by weight of 4-propyleneoxy-2-hydroxybenzophenone and 0.1-0.3 parts by weight of potassium persulfate to 60-80 parts by weight of deionized water, stirring at 70-80° C. for 8-10 hours, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 50-70° C. until constant weight, to obtain component C;
[0011] Step D: Add the component C, 0.3-0.5 parts by weight of vinyltrimethoxysilane and 1-2 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, and then stir in the dark at 60-70° C. for 14-16 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 50-70° C. until constant weight, and the preparation is completed.
[0012] Furthermore, the pH of the Tris-HCl buffer in step A is 8.5.
[0013] Furthermore, the power of the ultrasound in step A is 300-450W.
[0014] As a preferred technical solution of the present invention, the antioxidant is antioxidant 4010NA.
[0015] As a preferred technical solution of the present invention, the accelerator is a mixture of accelerator TMTD and accelerator DTDM; the mass ratio of the accelerator TMTD to the accelerator DTDM is 1-2:1.5-2.
[0016] As a preferred technical solution of the present invention, the vulcanizing agent is a mixture of sulfur and dicumyl peroxide; the mass ratio of the sulfur to the dicumyl peroxide is 0.5-0.8:2.
[0017] A method for preparing a high-pressure and weather-resistant EPDM rubber material, the method comprising the following steps:
[0018] (1) EPDM rubber and silicone rubber are first mixed at 150-155° C. for 60-90 minutes, and then modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer are added, and the mixing is continued at a constant temperature for 10-15 minutes, and the mixture is naturally cooled to room temperature to obtain a mixed rubber material;
[0019] (2) The mixed rubber material is vulcanized to complete the preparation.
[0020] Furthermore, the vulcanization temperature in step (2) is 170-180° C.; the vulcanization time is 15-30 min; and the vulcanization pressure is 10-15 MPa.
[0021] Beneficial effects of the present invention:
[0022] (1) The present invention first polymerizes and coats hexagonal boron nitride with dopamine hydrochloride to form an organic polymer interface, then adds vinyl trimethoxy silane to complete the first alkenyl modification, then uses 4-propyleneoxy-2-hydroxybenzophenone as a voltage stabilizer to polymerize via double bonds to achieve surface grafting of the voltage stabilizer, and finally further adds vinyl trimethoxy silane to complete the second alkenyl modification, thereby preparing a modified functional filler, which is then mixed with conventional components such as ethylene propylene diene rubber, silicone rubber, carbon black, paraffin oil, and antioxidants, and then vulcanized to obtain a new type of ethylene propylene diene rubber material, which not only has excellent high voltage resistance, but also has good weathering resistance, and is very suitable for use in the field of insulators.
[0023] (2) The present invention creatively prepares a modified functional filler by sequentially performing polymerization coating of dopamine hydrochloride, first alkenyl modification of vinyltrimethoxysilane, surface grafting of 4-propyleneoxy-2-hydroxybenzophenone, and second alkenyl modification of vinyltrimethoxysilane based on the advantages of high breakdown strength and low dielectric loss of hexagonal boron nitride itself. The inorganic interface of hexagonal boron nitride can be transformed into an organic interface through polymerization coating of dopamine hydrochloride, which enhances its compatibility in the EPDM rubber matrix to a certain extent. At the same time, a large number of hydroxyl groups and imino groups are provided. The hydroxyl groups can provide sites for further processing, while the imino groups mainly play a role in competing for free radicals in the aging process. After being combined with a small amount of antioxidant, the chain reaction can be terminated well, achieving the effect of inhibiting aging; 4-propyleneoxy-2-hydroxybenzophenone, as a voltage stabilizer containing double bonds, can improve the breakdown strength by weakening the energy of electrons. After being grafted to the organic interface of the hexagonal boron nitride surface, its ability to capture electrons can be greatly improved through the benzene ring group of the organic interface, further promoting the improvement of high-voltage resistance; as for the second alkenyl modification of vinyltrimethoxysilane, its purpose is to enable the modified functional filler to participate in the vulcanization system in the subsequent process, which not only solves the migration problem in the background technology, but also has better dispersibility and more uniform distribution, and the technical effect achieved is also more excellent.
[0024] (3) The EPDM rubber material prepared by the present invention has excellent high-voltage resistance and is not broken down even at 400,000 volts. At the same time, it has good weather aging resistance. DETAILED DESCRIPTION
[0025] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0026] The EPDM rubber in all embodiments and comparative examples of the present invention is purchased directly from the market, purchased from Dow Chemical, USA, with the brand name 3722P; the silicone rubber is purchased directly from the market, purchased from Dongjue Silicone Group Co., Ltd., with the model number 112-0; the hexagonal boron nitride is purchased directly from the market, purchased from Zhejiang Yamei Nano Technology Co., Ltd., with the product number AM-HBN-073-2; the carbon black is purchased directly from the market, purchased from Jinan Zhongbei Fine Chemical Co., Ltd., with the model number N550; the paraffin oil is purchased directly from the market, purchased from Changzhou Zhongke Synthetic Materials Co., Ltd., with the product specification of P300#.
[0027] Example 1
[0028] The invention discloses an EPDM rubber material which is resistant to high pressure and weathering. The EPDM rubber material is prepared from EPDM rubber, silicone rubber, modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer.
[0029] The mass ratio of the EPDM rubber, the silicone rubber, the modified functional filler, the carbon black, the paraffin oil, the antioxidant, the accelerator and the vulcanizer is 100:35:8:50:15:0.2:1:3.
[0030] The modified functional filler is prepared by the following steps:
[0031] Step A: adding 1 part by weight of dopamine hydrochloride and 2 parts by weight of hexagonal boron nitride to 120 parts by weight of Tris-HCl buffer, and then stirring the mixture ultrasonically at 30° C. for 10 hours in contact with air, filtering, taking the filter residue, washing it with deionized water, and finally drying it in vacuum at 50° C. until constant weight, to obtain component A;
[0032] Step B: Add the component A, 0.5 parts by weight of vinyltrimethoxysilane and 1 part by weight of deionized water to 100 parts by weight of anhydrous ethanol, and then stir at 60° C. in the dark for 14 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 50° C. until constant weight, to obtain component B;
[0033] Step C: adding 20 parts by weight of dimethyl sulfoxide, the component B, 1 part by weight of 4-propyleneoxy-2-hydroxybenzophenone and 0.1 part by weight of potassium persulfate to 60 parts by weight of deionized water, and then stirring at 70° C. for 8 hours, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 50° C. until constant weight, to obtain component C;
[0034] Step D: Add the component C, 0.3 parts by weight of vinyltrimethoxysilane and 1 part by weight of deionized water to 100 parts by weight of anhydrous ethanol, then stir in the dark at 60° C. for 14 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 50° C. until constant weight, and the preparation is completed.
[0035] The pH of the Tris-HCl buffer in step A is 8.5.
[0036] The power of the ultrasound in step A is 300W.
[0037] The antioxidant is antioxidant 4010NA.
[0038] The accelerator is formed by mixing accelerator TMTD and accelerator DTDM; the mass ratio of the accelerator TMTD to the accelerator DTDM is 1:1.5.
[0039] The vulcanizing agent is a mixture of sulfur and dicumyl peroxide; the mass ratio of the sulfur to the dicumyl peroxide is 0.5:2.
[0040] A method for preparing a high-pressure and weather-resistant EPDM rubber material, the method comprising the following steps:
[0041] (1) EPDM rubber and silicone rubber are first mixed at 150° C. for 60 minutes, and then modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer are added, and the mixture is mixed at a constant temperature for 10 minutes, and then naturally cooled to room temperature to obtain a mixed rubber material;
[0042] (2) The mixed rubber material is vulcanized to complete the preparation.
[0043] The vulcanization temperature of step (2) is 170° C.; the vulcanization time is 15 min; and the vulcanization pressure is 10 MPa.
[0044] Example 2
[0045] The invention discloses an EPDM rubber material which is resistant to high pressure and weathering. The EPDM rubber material is prepared from EPDM rubber, silicone rubber, modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer.
[0046] The mass ratio of the EPDM rubber, the silicone rubber, the modified functional filler, the carbon black, the paraffin oil, the antioxidant, the accelerator and the vulcanizer is 100:40:10:55:15:0.2:1.5:3.
[0047] The modified functional filler is prepared by the following steps:
[0048] Step A: adding 1.5 parts by weight of dopamine hydrochloride and 2.5 parts by weight of hexagonal boron nitride to 140 parts by weight of Tris-HCl buffer, and then stirring the mixture ultrasonically at 40° C. for 12 hours in contact with air, filtering, taking the filter residue, washing it with deionized water, and finally drying it in vacuum at 70° C. until constant weight, to obtain component A;
[0049] Step B: Add the component A, 1 part by weight of vinyltrimethoxysilane and 2 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, and then stir at 70° C. in the dark for 16 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 70° C. until constant weight, to obtain component B;
[0050] Step C: adding 30 parts by weight of dimethyl sulfoxide, the component B, 1.5 parts by weight of 4-propyleneoxy-2-hydroxybenzophenone and 0.3 parts by weight of potassium persulfate to 80 parts by weight of deionized water, and then stirring at 80° C. for 10 hours, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 70° C. until constant weight, to obtain component C;
[0051] Step D: Add the component C, 0.5 parts by weight of vinyltrimethoxysilane and 2 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, then stir in the dark at 70° C. for 16 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 70° C. until constant weight, and the preparation is completed.
[0052] The pH of the Tris-HCl buffer in step A is 8.5.
[0053] The power of the ultrasound in step A is 450W.
[0054] The antioxidant is antioxidant 4010NA.
[0055] The accelerator is formed by mixing accelerator TMTD and accelerator DTDM; the mass ratio of the accelerator TMTD to the accelerator DTDM is 2:2.
[0056] The vulcanizing agent is a mixture of sulfur and dicumyl peroxide; the mass ratio of the sulfur to the dicumyl peroxide is 0.8:2.
[0057] A method for preparing a high-pressure and weather-resistant EPDM rubber material, the method comprising the following steps:
[0058] (1) EPDM rubber and silicone rubber are first mixed at 155° C. for 90 minutes, and then modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer are added, and the mixture is mixed at a constant temperature for 15 minutes, and then naturally cooled to room temperature to obtain a mixed rubber material;
[0059] (2) The mixed rubber material is vulcanized to complete the preparation.
[0060] The vulcanization temperature of step (2) is 180° C.; the vulcanization time is 30 min; and the vulcanization pressure is 15 MPa.
[0061] Example 3
[0062] The invention discloses an EPDM rubber material which is resistant to high pressure and weathering. The EPDM rubber material is prepared from EPDM rubber, silicone rubber, modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer.
[0063] The mass ratio of the EPDM rubber, the silicone rubber, the modified functional filler, the carbon black, the paraffin oil, the antioxidant, the accelerator and the vulcanizer is 100:38:9:53:15:0.2:1.3:3.
[0064] The modified functional filler is prepared by the following steps:
[0065] Step A: adding 1.3 parts by weight of dopamine hydrochloride and 2.2 parts by weight of hexagonal boron nitride to 130 parts by weight of Tris-HCl buffer, and then stirring the mixture ultrasonically at 35° C. for 11 hours in contact with air, filtering, taking the filter residue, washing it with deionized water, and finally drying it in vacuo at 60° C. until constant weight, to obtain component A;
[0066] Step B: Add the component A, 0.8 parts by weight of vinyltrimethoxysilane and 1.5 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, and then stir at 65° C. in the dark for 15 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 60° C. until constant weight, to obtain component B;
[0067] Step C: adding 25 parts by weight of dimethyl sulfoxide, the component B, 1.3 parts by weight of 4-propyleneoxy-2-hydroxybenzophenone and 0.2 parts by weight of potassium persulfate to 70 parts by weight of deionized water, and then stirring at 75° C. for 9 hours, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 60° C. until constant weight, to obtain component C;
[0068] Step D: Add the component C, 0.4 parts by weight of vinyltrimethoxysilane and 1.5 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, then stir in the dark at 65° C. for 15 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 65° C. until constant weight, and the preparation is completed.
[0069] The pH of the Tris-HCl buffer in step A is 8.5.
[0070] The power of the ultrasound in step A is 400W.
[0071] The antioxidant is antioxidant 4010NA.
[0072] The accelerator is a mixture of accelerator TMTD and accelerator DTDM; the mass ratio of the accelerator TMTD to the accelerator DTDM is 1.5:1.8.
[0073] The vulcanizing agent is a mixture of sulfur and dicumyl peroxide; the mass ratio of the sulfur to the dicumyl peroxide is 0.7:2.
[0074] A method for preparing a high-pressure and weather-resistant EPDM rubber material, the method comprising the following steps:
[0075] (1) EPDM rubber and silicone rubber were first mixed at 153° C. for 80 min, and then modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer were added, and the mixture was mixed at constant temperature for 13 min, and then naturally cooled to room temperature to obtain a mixed rubber material;
[0076] (2) The mixed rubber material is vulcanized to complete the preparation.
[0077] The vulcanization temperature of step (2) is 175° C.; the vulcanization time is 25 min; and the vulcanization pressure is 13 MPa.
[0078] Comparative Example 1
[0079] On the basis of Example 1, the dopamine hydrochloride in step A was changed to 0.6 parts by weight, and the rest remained unchanged.
[0080] Comparative Example 2
[0081] Based on Example 1, the vinyltrimethoxysilane in step D was replaced with an equal weight of deionized water, and the rest remained unchanged.
[0082] Comparative Example 3
[0083] On the basis of Example 1, step C and step D are not performed, and step B is changed to adding component A, 0.3 parts by weight of vinyltrimethoxysilane and 1 part by weight of deionized water to 100 parts by weight of anhydrous ethanol, and then stirring at 60° C. in the dark for 14 hours, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 50° C. until constant weight to obtain component B, and adding 1 part by weight of 4-propyleneoxy-2-hydroxybenzophenone to component B, that is, the preparation is completed; the rest remains unchanged.
[0084] Comparative Example 4
[0085] On the basis of Example 1, the mass ratio of the EPDM rubber, the silicone rubber, the modified functional filler, the carbon black, the paraffin oil, the antioxidant, the accelerator and the vulcanizer is changed to 100:35:8:50:15:1:1:3, and the rest remain unchanged.
[0086] Comparative Example 5
[0087] Based on Example 1, no antioxidant was added in step (1), and the rest remained unchanged.
[0088] Comparative Example 6
[0089] On the basis of Example 1, step D was omitted, the amount of vinyltrimethoxysilane in step B was changed to 0.8 parts by weight, and the rest remained unchanged.
[0090] Test Example 1
[0091] High voltage resistance test:
[0092] The EPDM rubber materials prepared in Examples 1-3 and Comparative Examples 1-6 were respectively subjected to breakdown voltage strength tests according to the reference standard GB / T 1695-2005, wherein the temperature during the test was 30° C. and the results were rounded off to integers.
[0093] Table 1. High voltage resistance test results
[0094] Breakdown voltage strength / kV / mm Example 1 407 Example 2 405 Example 3 409 Comparative Example 1 381 Comparative Example 2 367 Comparative Example 3 374 Comparative Example 4 406 Comparative Example 5 406 Comparative Example 6 365
[0095] Test Example 2
[0096] Weathering resistance test:
[0097] The EPDM rubber materials prepared in Examples 1-3 and Comparative Examples 1-6 were aged at 100° C. for 20 days, cooled naturally to room temperature, and then the breakdown voltage strength test in Test Example 1 was repeated to illustrate the weather aging resistance effect.
[0098] Table 2. Weathering resistance test results
[0099]
[0100]
[0101] Comparison between Example 1 and Comparative Examples 1-6 shows that:
[0102] The difference between Comparative Example 1 and Example 1 is that the amount of dopamine hydrochloride used is reduced, and correspondingly, the groups that can be provided are reduced.
[0103] The difference between Comparative Example 2 and Example 1 is that no second olefin modification is performed.
[0104] The difference between Comparative Example 3 and Example 1 is that 4-propyleneoxy-2-hydroxybenzophenone is not grafted onto the organic interface of the hexagonal boron nitride surface.
[0105] The difference between Comparative Example 4 and Example 1 is that the amount of antioxidant used is increased.
[0106] The difference between Comparative Example 5 and Example 1 is that no antioxidant is added.
[0107] The difference between Comparative Example 6 and Example 1 is that no second alkenyl modification is performed, and at the same time, the amount of vinyltrimethoxysilane used in the first alkenyl modification is increased.
[0108] From the comparison of test examples 1-2 and example 1 and comparative examples 1-6, it can be seen that the EPDM rubber material prepared by the present invention not only has excellent high pressure resistance, but also has good weather aging resistance. Only a small amount of antioxidant is needed in the component to achieve a good anti-aging effect, which greatly saves production costs.
[0109] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. An EPDM rubber material resistant to high pressure and weathering, characterized in that: The EPDM rubber material is prepared from EPDM rubber, silicone rubber, modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer.
2. The high pressure and weather aging resistant EPDM rubber material according to claim 1, characterized in that: The mass ratio of the EPDM rubber, the silicone rubber, the modified functional filler, the carbon black, the paraffin oil, the antioxidant, the accelerator and the vulcanizer is 100:35-40:8-10:50-55:15:0.2:1-1.5:
3.
3. The high pressure and weather aging resistant EPDM rubber material according to claim 1, characterized in that: The modified functional filler is prepared by the following steps: Step A: adding 1-1.5 parts by weight of dopamine hydrochloride and 2-2.5 parts by weight of hexagonal boron nitride to 120-140 parts by weight of Tris-HCl buffer, and then stirring ultrasonically at 30-40° C. for 10-12 hours in contact with air, filtering, taking the filter residue, washing it with deionized water, and finally vacuum drying it at 50-70° C. until constant weight, to obtain component A; Step B: adding the component A, 0.5-1 parts by weight of vinyltrimethoxysilane and 1-2 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, stirring for 14-16 hours at 60-70° C. in the dark, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 50-70° C. until constant weight, to obtain component B; Step C: adding 20-30 parts by weight of dimethyl sulfoxide, the component B, 1-1.5 parts by weight of 4-propyleneoxy-2-hydroxybenzophenone and 0.1-0.3 parts by weight of potassium persulfate to 60-80 parts by weight of deionized water, stirring at 70-80° C. for 8-10 hours, filtering, taking the filter residue, washing with deionized water, and finally vacuum drying at 50-70° C. until constant weight, to obtain component C; Step D: Add the component C, 0.3-0.5 parts by weight of vinyltrimethoxysilane and 1-2 parts by weight of deionized water to 100 parts by weight of anhydrous ethanol, and then stir in the dark at 60-70° C. for 14-16 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 50-70° C. until constant weight, and the preparation is completed.
4. The high pressure and weather aging resistant EPDM rubber material according to claim 3, characterized in that: The pH of the Tris-HCl buffer in step A is 8.
5.
5. The high pressure and weather aging resistant EPDM rubber material according to claim 3, characterized in that: The power of the ultrasound in step A is 300-450W.
6. The high pressure and weather aging resistant EPDM rubber material according to claim 1, characterized in that: The antioxidant is antioxidant 4010NA.
7. The high pressure and weather aging resistant EPDM rubber material according to claim 1, characterized in that: The accelerator is formed by mixing accelerator TMTD and accelerator DTDM; the mass ratio of the accelerator TMTD to the accelerator DTDM is 1-2:1.5-2.
8. The high pressure and weather aging resistant EPDM rubber material according to claim 1, characterized in that: The vulcanizing agent is a mixture of sulfur and dicumyl peroxide; the mass ratio of the sulfur to the dicumyl peroxide is 0.5-0.8:
2.
9. A method for preparing a high pressure and weathering resistant EPDM rubber material according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: (1) EPDM rubber and silicone rubber are first mixed at 150-155° C. for 60-90 minutes, and then modified functional filler, carbon black, paraffin oil, antioxidant, accelerator and vulcanizer are added, and the mixing is continued at a constant temperature for 10-15 minutes, and the mixture is naturally cooled to room temperature to obtain a mixed rubber material; (2) The mixed rubber material is vulcanized to complete the preparation.
10. The method for preparing a high pressure and weather aging resistant EPDM rubber material according to claim 9, characterized in that: The vulcanization temperature in step (2) is 170-180° C.; the vulcanization time is 15-30 min; and the vulcanization pressure is 10-15 MPa.
Citation Information
Patent Citations
Heat aging-resisting and low-pressure change sulfur vulcanized EPDM (Ethylene-Propylene-Diene Monomer) rubber composition, preparation method, application and application product thereof
CN107189236A
High-voltage cable stabilizer and preparation method thereof
CN111286082A
Anti-aging corrosion-resistant battery backboard and preparation method thereof
CN115558345A
Arc-resistant silicon rubber composite material, preparation method, and uses thereof
WO2016206243A1
Cited By
High and low temperature resistant ethylene propylene rubber base material and preparation method thereof
CN120399361A
Anti-aging composite silicone rubber material and preparation method thereof
CN121160094A