Antibacterial nylon and preparation method thereof

By using concave and convex rod soil-nano silver composite powder in nylon materials, the problem of traditional nylon materials lacking antibacterial properties is solved, the significance and durability of the antibacterial effect is achieved, and the drug resistance is avoided. The process is simple, environmentally friendly and safe. Suitable for industrial production.

CN119060533AInactive Publication Date: 2024-12-03NANJING LIHUA ENG PLASTIC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411309024.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional nylon materials lack antibacterial properties. In the existing antibacterial nylon preparation methods, antibacterial agents are unevenly dispersed, unstable, and easy to develop drug resistance.

Method used

The concave and convex rod soil-nano-silver composite inorganic powder is used. The mass ratio of nano-silver to concave and concave and convex rod soil is within the range of 10:100 to 100:100, and the nano-silver particle size is controlled at 3-100nm. Combined with nylon resin for melt blending to ensure The uniform dispersion and stability of antibacterial agents.

Benefits of technology

It achieves the significance and durability of the antibacterial effect, avoids the occurrence of drug resistance, and has environmentally friendly and safe processes, which are suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an antibacterial nylon and a preparation method thereof, the antibacterial nylon is composed of a nylon resin matrix and an antibacterial agent uniformly dispersed in the nylon resin matrix, the antibacterial agent is attapulgite-nano silver composite inorganic powder, the mass ratio of nano silver to attapulgite is accurately controlled in a range of 10: 100-100: 100, and the antibacterial agent is nano silver-nano silver composite inorganic powder. The particle size of the nano-silver is strictly controlled to be 3-100 nm, so that the optimal antibacterial effect and stability are ensured; according to the invention, the attapulgite and the nano-silver are compounded, the antibacterial property of the nano-silver is utilized, and the good dispersibility of the attapulgite is combined, so that the antibacterial agent is uniformly dispersed in a nylon matrix, the antibacterial effect is remarkable and lasting, and drug resistance is not generated; the use of an organic solvent is avoided, the emission of environmental pollutants is reduced, and the antibacterial agent does not separate out harmful substances and is friendly to a human body and the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to an antibacterial nylon and a preparation method thereof. Background Art

[0002] As people's requirements for quality of life increase, the demand for antibacterial materials is increasing. Nylon, as an important polymer material, is widely used in many fields. However, traditional nylon materials themselves do not have antibacterial properties and are difficult to meet the antibacterial requirements in specific fields. In the prior art, methods for preparing antibacterial nylon by adding antibacterial agents have been widely studied, such as adding silver ions, nano zinc oxide, organic antibacterial agents, etc. However, these methods have problems such as uneven dispersion of antibacterial agents, unstable antibacterial effects, and easy development of drug resistance. Therefore, it is of great significance to develop an antibacterial nylon with significant, long-lasting and stable antibacterial effect and a preparation method thereof. To this end, the present invention proposes an antibacterial nylon and a preparation method thereof. Summary of the invention

[0003] The object of the present invention is to provide an antibacterial nylon and a preparation method thereof, so as to solve the problems of uneven dispersion of antibacterial agents, unstable antibacterial effects and easy generation of drug resistance in the existing antibacterial nylon preparation process.

[0004] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: an antibacterial nylon, which is composed of a nylon resin matrix and an antibacterial agent uniformly dispersed therein, wherein the antibacterial agent is a attapulgite-nanosilver composite inorganic powder, wherein the mass ratio of nanosilver to attapulgite is precisely controlled within the range of 10:100 to 100:100, and the particle size of nanosilver is strictly controlled between 3-100nm to ensure the best antibacterial effect and stability.

[0005] Preferably, the attapulgite has a natural rod-like or fibrous structure, and the diameter of the rod crystal is between 10-80 nm, which provides abundant attachment points for nanosilver. The nanosilver particles are uniformly adsorbed on the surface of the attapulgite in a spherical shape to form a tight bond, thereby avoiding the agglomeration of the nanosilver and improving its dispersibility and stability in the nylon matrix.

[0006] Preferably, the weight ratio of the attapulgite-nanosilver composite inorganic powder to the nylon resin is precisely controlled within the range of (0.01-1):100, preferably (0.01-0.1):100, so as to ensure the antibacterial effect without affecting the mechanical properties and processing properties of the nylon material.

[0007] The present invention also provides a method for preparing the above-mentioned antibacterial nylon, which comprises the following specific steps:

[0008] Step 1, preparation of attapulgite suspension: accurately weighed attapulgite and deionized water are mixed in a mass ratio of 1:10 to 1:20, and stirred in a reactor equipped with a stirrer. The stirring speed and time must be sufficient to fully disperse the attapulgite to form a uniform attapulgite suspension;

[0009] Step 2: Nanosilver loading: Add accurately weighed silver nitrate to the attapulgite suspension prepared in step 1, and stir the mixture at a temperature of 50-90° C. and a stirring speed of 100-500 rpm. The reaction time should be sufficient to allow the nanosilver particles to be evenly loaded on the surface of the attapulgite.

[0010] Step 3, spray drying: spray drying the attapulgite-nanosilver suspension obtained in step 2 through a spray dryer, and the temperature and pressure of the spray drying need to be precisely controlled to obtain attapulgite-nanosilver composite inorganic powder with uniform particle size and good dispersibility;

[0011] Step 4, melt blending: melt blending the attapulgite-nanosilver composite inorganic powder obtained in step 3 and the nylon resin in a ratio of (0.01-0.1):100. The melt blending temperature needs to be higher than the melting point of the nylon resin but avoid being too high to cause degradation. The blending time needs to be sufficient to evenly disperse the antibacterial agent in the nylon matrix to obtain the antibacterial nylon.

[0012] Preferably, in step 1, the attapulgite needs to be subjected to a thermal activation treatment to improve its surface activity and dispersibility, and the thermal activation treatment conditions are heating treatment at a temperature of 250-350° C. for 1-3 hours.

[0013] Preferably, in step 2, the amount of silver nitrate added needs to be accurately calculated according to the required loading amount of nanosilver, and the particle size and distribution of the nanosilver particles are controlled by adjusting the reaction temperature and stirring speed.

[0014] Preferably, in step three, the inlet temperature and outlet temperature of the spray dryer need to be accurately set to ensure the drying effect and particle size distribution of the attapulgite-nanosilver composite inorganic powder.

[0015] Preferably, in step 4, the temperature of melt blending needs to be adjusted according to the specific model and properties of the nylon resin to ensure sufficient melting of the nylon resin and uniform dispersion of the antibacterial agent. At the same time, appropriate amounts of antioxidants, lubricants and other additives can be added during the melt blending process to improve the processing properties of the nylon material and the performance of the final product.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. Significant and lasting antibacterial effect: The present invention combines attapulgite with nano-silver, utilizes the antibacterial property of nano-silver, and combines the good dispersibility of attapulgite to make the antibacterial agent evenly dispersed in the nylon matrix, and the antibacterial effect is significant and lasting.

[0018] 2. No drug resistance: Nano-silver antibacterial agents achieve antibacterial purposes by slowly releasing silver ions, and are not likely to cause bacteria to develop drug resistance.

[0019] 3. Environmental protection and safety: The present invention avoids the use of organic solvents, reduces the emission of environmental pollutants, and the antibacterial agent does not precipitate harmful substances, which is friendly to the human body and the environment.

[0020] 4. Simple process and easy implementation: The preparation method of the present invention is simple, the raw materials are easily available, and it is convenient for industrial production. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] This is the first embodiment of the present invention, which provides a solution:

[0024] 1. Preparation of attapulgite suspension:

[0025] Raw materials: 100 g of thermally activated attapulgite (heating treatment at 300° C. for 2 hours) and 1000 mL of deionized water.

[0026] Equipment: Use a reactor with a capacity of at least 1.5 L and equipped with a stirrer and temperature control system.

[0027] step:

[0028] a. Clean the reactor and preheat it to room temperature.

[0029] b. 100 g of heat-activated attapulgite was slowly added into the reactor, and the stirrer was turned on at a stirring speed of 300 rpm.

[0030] c. Slowly add 1000 mL of deionized water to the reactor while continuing to stir to ensure that the attapulgite is fully dispersed.

[0031] d. Set the stirring time to 30 minutes, keep the stirring speed constant during this period, and observe the state of the suspension to ensure that there is no agglomeration.

[0032] e. After the stirring is completed, turn off the stirrer and the temperature control system to obtain a uniform attapulgite suspension.

[0033] 2. Nanosilver loading:

[0034] Raw materials: 10g silver nitrate.

[0035] Equipment: Same as the reactor in step 1, but make sure there are no other impurities left.

[0036] step:

[0037] a. The attapulgite suspension prepared in step 1 was reheated to 70°C, the stirrer was turned on, and the stirring speed was set to 200 rpm.

[0038] b. Slowly add 10 g of silver nitrate to the suspension while continuing to stir to ensure that the silver nitrate is evenly dispersed.

[0039] c. Maintain the reaction temperature at 70°C and set the stirring time to 6 hours. During this time, observe the color change of the reaction solution. Usually, the solution will appear slightly yellow after the nanosilver is generated.

[0040] d. After the reaction is completed, turn off the agitator and temperature control system and allow the suspension to cool naturally to room temperature.

[0041] 3. Spray drying:

[0042] Equipment: Use industrial-grade spray dryer equipped with inlet air temperature, outlet air temperature and spray pressure adjustment system.

[0043] step:

[0044] a. Preheat the spray dryer to an inlet temperature of 180°C and an outlet temperature of 80°C.

[0045] b. The attapulgite-nanosilver suspension obtained in step 2 is fed into the nozzle of a spray dryer via a peristaltic pump or a high-pressure pump, and the spray pressure is set to 0.2 MPa.

[0046] c. During the spray drying process, observe the powder state at the outlet to ensure that there is no agglomeration and the drying is uniform.

[0047] d. After drying, the powder at the outlet of the spray dryer is collected, which is the attapulgite-nanosilver composite inorganic powder.

[0048] 4. Melt blending:

[0049] Raw materials: 100 g of nylon resin PA6, 1 g of the attapulgite-nanosilver composite inorganic powder obtained in step 3.

[0050] Equipment: Twin-screw extruder, equipped with temperature control system and screw speed adjustment system.

[0051] step:

[0052] a. Preheat the twin-screw extruder to 230°C and set the screw speed to 200 rpm.

[0053] b. After the nylon resin and attapulgite-nanosilver composite inorganic powder are mixed evenly in proportion, the mixture is added into the hopper of the extruder.

[0054] c. Start the extruder and observe the melting and mixing of the material in the screw to ensure there is no blockage.

[0055] d. The melt blending time was set to 10 minutes, during which the temperature and rotation speed were kept constant.

[0056] e. After melt blending, the antibacterial nylon strips are extruded through the die head of the extruder and cut into the required length after cooling.

[0057] Example 2

[0058] This is the second embodiment of the present invention, which is based on the previous embodiment, except that:

[0059] 2. Nanosilver loading:

[0060] Raw materials: 50g silver nitrate.

[0061] step:

[0062] b. Slowly add 50 g of silver nitrate to the suspension, and the remaining steps are the same as in Example 1.

[0063] 3. Spray drying:

[0064] Equipment: Same as Example 1, but the scale of the spray dryer may need to be adjusted according to the output.

[0065] step:

[0066] a. Preheat the spray dryer to an inlet temperature of 200°C and an outlet temperature of 90°C. The remaining steps are the same as in Example 1.

[0067] 4. Melt blending:

[0068] Raw materials: nylon resin PA66 100g, attapulgite-nanosilver composite inorganic powder 0.1g.

[0069] step:

[0070] a. Preheat the twin-screw extruder to 260°C, set the screw speed to 150 rpm, and the remaining steps are the same as in Example 1.

[0071] Although embodiments of the present invention have been shown and described (see the above detailed description for details), it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An antibacterial nylon, characterized in that: The antibacterial nylon is composed of a nylon resin matrix and an antibacterial agent uniformly dispersed therein, wherein the antibacterial agent is a attapulgite-nanosilver composite inorganic powder, wherein the mass ratio of nanosilver to attapulgite is precisely controlled within the range of 10:100 to 100:100, and the particle size of the nanosilver is strictly controlled between 3-100nm to ensure the best antibacterial effect and stability.

2. The antibacterial nylon according to claim 1, characterized in that: The attapulgite has a natural rod-like or fibrous structure, and the diameter of the rod crystal is between 10-80nm, which provides abundant attachment points for nanosilver. The nanosilver particles are uniformly adsorbed on the surface of the attapulgite in a spherical shape to form a tight bond, thereby avoiding the agglomeration of the nanosilver and improving its dispersibility and stability in the nylon matrix.

3. The antibacterial nylon according to claim 1 or 2, characterized in that: The weight ratio of the attapulgite-nanosilver composite inorganic powder to the nylon resin is precisely controlled within the range of (0.01-1):100, preferably (0.01-0.1):100, so as to ensure the antibacterial effect while not affecting the mechanical properties and processing properties of the nylon material.

4. A method for preparing the antibacterial nylon according to any one of claims 1 to 3, characterized in that: The method comprises the following specific steps: Step 1, preparation of attapulgite suspension: accurately weighed attapulgite and deionized water are mixed in a mass ratio of 1:10 to 1:20, and stirred in a reactor equipped with a stirrer. The stirring speed and time must be sufficient to fully disperse the attapulgite to form a uniform attapulgite suspension; Step 2: Nanosilver loading: Add accurately weighed silver nitrate to the attapulgite suspension prepared in step 1, and stir the mixture at a temperature of 50-90° C. and a stirring speed of 100-500 rpm. The reaction time should be sufficient to allow the nanosilver particles to be evenly loaded on the surface of the attapulgite. Step 3, spray drying: spray drying the attapulgite-nanosilver suspension obtained in step 2 through a spray dryer, and the temperature and pressure of the spray drying need to be precisely controlled to obtain attapulgite-nanosilver composite inorganic powder with uniform particle size and good dispersibility; Step 4, melt blending: melt blending the attapulgite-nanosilver composite inorganic powder obtained in step 3 and the nylon resin in a ratio of (0.01-0.1):

100. The melt blending temperature needs to be higher than the melting point of the nylon resin but avoid being too high to cause degradation. The blending time needs to be sufficient to evenly disperse the antibacterial agent in the nylon matrix to obtain the antibacterial nylon.

5. The preparation method according to claim 4, characterized in that: In step 1, the attapulgite needs to be subjected to heat activation treatment to improve its surface activity and dispersibility. The heat activation treatment condition is heating treatment at a temperature of 250-350° C. for 1-3 hours.

6. The preparation method according to claim 4, characterized in that: In step 2, the amount of silver nitrate added needs to be accurately calculated according to the required loading amount of nanosilver, and the particle size and distribution of the nanosilver particles are controlled by adjusting the reaction temperature and stirring speed.

7. The preparation method according to claim 4, characterized in that: In step three, the inlet temperature and outlet temperature of the spray dryer must be accurately set to ensure the drying effect and particle size distribution of the attapulgite-nanosilver composite inorganic powder.

8. The preparation method according to claim 4, characterized in that: In step 4, the temperature of melt blending needs to be adjusted according to the specific type and properties of the nylon resin to ensure sufficient melting of the nylon resin and uniform dispersion of the antibacterial agent. At the same time, appropriate amounts of antioxidants, lubricants and other additives can be added during the melt blending process to improve the processing properties of the nylon material and the performance of the final product.

Citation Information

Patent Citations

  • Antibacterial nylon and a preparing method thereof

    CN106633829A