Optical fiber array silica gel protective cap and preparation method thereof

By designing the formula and process flow of silicone impregnation liquid, an optical fiber array silicone protective cap that can maintain performance under high and low temperature cycle conditions was prepared, which solved the problem of easy degumming of existing optical fiber array silicone protective caps and realized the FA fiber Effective protection of connectors.

CN119060543APending Publication Date: 2024-12-03FOSHAN FANGPU PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202191.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing fiber array silicone protective caps are prone to degumming during use, resulting in damage to the fiber connector, and cannot meet the high temperature resistance requirements, and cannot effectively protect the processing and packaging process of FA products.

Method used

The fiber array silicone protective cap is used for fiber-based array prepared from silicone impregnation liquid. The silicone impregnation liquid is composed of vinyl silicone oil, white carbon black, surface treatment agent, deionized water, silicone resin, hydrogen-containing silicone oil, fluorine-containing filler, inhibitor and catalyst. A high-performance protective cap is formed through specific formula ratios and process flow to ensure that there is no adhesion and degumming under high and low temperature cycle conditions.

Benefits of technology

The obtained fiber array silicone protective cap performs well in terms of hardness, tensile strength, tear strength and elongation of break. It can maintain performance after 10 cycles at high and low temperatures, effectively protect FA fiber connectors, and avoid adhesion and degumming problems. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060543A_ABST
    Figure CN119060543A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of silica gel materials, and discloses an optical fiber array silica gel protective cap and a preparation method thereof.The optical fiber array silica gel protective cap is formed by impregnating a mold with silica gel impregnation liquid and curing the silica gel impregnation liquid, and the silica gel impregnation liquid is prepared from, by weight, 50-250 parts of vinyl silicone oil, 10-40 parts of white carbon black and 1-5 parts of surface treating agent; the invention discloses a high-temperature-resistant coating which is prepared from the following components in parts by weight: 1-5 parts of deionized water, 5-20 parts of silicon resin, 5-35 parts of hydrogen-containing silicone oil, 1-10 parts of fluorine-containing filler, 0.1-3 parts of inhibitor and 0.05-0.6 part of catalyst. According to the invention, the formula of the silica gel impregnation liquid is designed, and the optical fiber array silica gel protective cap used for protecting the FA optical fiber connector is prepared based on the silica gel impregnation liquid; the optical fiber array silica gel protective cap prepared by the invention has better physical properties such as hardness, tensile strength, tear strength and elongation at break, does not have the phenomenon of adhesion and degumming after 10 times of high and low temperature circulation, and can be effectively used for processing and protecting FA optical fiber connector products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicone materials, and in particular relates to an optical fiber array silicone protective cap and a preparation method thereof. Background Art

[0002] As optical communications develop towards high speed and integration, optical transceiver modules also need to adopt smaller and more integrated solutions, which has led to a rapid increase in the demand for high-speed optical components. With the rapid advancement of 400G and 800G high-speed transmission, high-density and small-volume FA (fiber array) is a more ideal solution. FA fiber array is most commonly used for the packaging of planar waveguide splitters (PLC) and arrayed waveguide gratings (AWG). FA needs to go through a glue curing process during the assembly process. Generally, manufacturers will put on a protective cap for curing, so the protective cap is required to be resistant to high temperatures. The currently commonly used PVC protective cap material cannot meet this requirement.

[0003] In addition, the protective cap will not be removed until the FA product is processed and enters the optical module manufacturer for packaging. During this process, the protective cap will contact optical components such as FA component lenses and chips, so the protective cap is not allowed to have glue falling off or residual glue. However, the existing optical fiber array silicone protective cap will debond during use, which will corrode the optical fiber connector and UV glue; and the user needs to clean the optical fiber connector core after installation and use, which not only consumes extra time and increases costs, but also has the risk of damaging the connector.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a fiber optic array silicone protective cap and a preparation method thereof, aiming to solve the problem that the existing fiber optic array silicone protective cap is prone to degumming when used in FA product processing, thereby causing damage to the optical fiber connector.

[0006] The technical solution of the present invention is as follows:

[0007] A silicone protective cap for an optical fiber array, wherein the silicone protective cap for the optical fiber array is formed by impregnating a silicone impregnation liquid on a mold and curing the impregnation liquid, wherein the silicone impregnation liquid comprises, by weight: 50-250 parts of vinyl silicone oil, 10-40 parts of white carbon black, 1-5 parts of a surface treatment agent, 1-5 parts of deionized water, 5-20 parts of silicone resin, 5-35 parts of hydrogen-containing silicone oil, 1-10 parts of a fluorine-containing filler, 0.1-3 parts of an inhibitor, and 0.05-0.6 parts of a catalyst.

[0008] The optical fiber array silicone protective cap, wherein the vinyl silicone oil is composed of a mixture of terminal vinyl silicone oil with a viscosity of 5000mPa·s, terminal vinyl silicone oil with a viscosity of 500mPa·s and polyvinyl silicone oil in a weight ratio of (50-120):(20-60):(10-30).

[0009] The optical fiber array silicone protective cap, wherein the surface treatment agent is one or more of a silane coupling agent, a siloxane coupling agent and a silazane coupling agent.

[0010] The optical fiber array silicone protective cap, wherein the silicone resin is one or more of methyl silicone resin, low phenyl methyl silicone resin, fluorosilicone resin, methyl MQ silicone resin and vinyl MQ silicone resin.

[0011] The optical fiber array silicone protective cap, wherein the fluorine-containing filler is one or more of fluorine-containing nanomaterials, fluorine plastics and fluorine rubber.

[0012] The optical fiber array silicone protective cap, wherein the hydrogen-containing silicone oil is at least one of terminal hydrogen-containing silicone oil and silicone oil containing active hydrogen in both the terminal group and the side chain.

[0013] The optical fiber array silicone protective cap, wherein the inhibitor is one or more of acetylene alcohol compounds, polyvinyl polysiloxane and maleate compounds.

[0014] The optical fiber array silicone protective cap, wherein the catalyst is at least one of a platinum-vinylsiloxane complex and an alcohol-modified chloroplatinic acid complex.

[0015] The optical fiber array silicone protective cap, wherein the specific surface area of ​​the white carbon black is 150-300m 2 / g.

[0016] A method for preparing the optical fiber array silicone protective cap according to the present invention comprises the following steps:

[0017] S100, according to the proportion, put part of the terminal vinyl silicone oil with a viscosity of 5000mPa·s into the kneader, add half of the amount of white carbon black in batches, and knead at room temperature for 0.5-2h; continue kneading and add the remaining white carbon black, surface treatment agent and deionized water in batches during this process, and the kneader speed is 5-20 rpm; add the remaining total terminal vinyl silicone oil with a viscosity of 5000mPa·s and fluorine-containing filler, then heat to 80-150°C, and knead for 2-4h; finally evacuate, knead for 1-2h at a vacuum degree of 0.1-0.3MPa and a temperature of 120-150°C; add the terminal vinyl silicone oil and polyvinyl silicone oil with a viscosity of 500mPa·s in batches, knead for 1-3h, and the kneader speed is 10-30 rpm. After the stirring is completed, cool to room temperature, take out the rubber material and grind it to obtain a grinding product;

[0018] S200, putting the ground product into a planetary mixer, adding hydrogenated silicone oil in batches and stirring for 1-2 hours, adding an inhibitor and stirring for 0.5-2 hours, and finally adding a catalyst and stirring for 0.5-2 hours, with the mixer rotating at a speed of 50-80 rpm until the paste is evenly dispersed; after the stirring is completed, filtering with a sieve and degassing to obtain a silica gel impregnation solution;

[0019] S300, preheating the optical fiber array silicone protective cap mold at 200-370°C for 30-100s;

[0020] S400, immersing the preheated optical fiber array silicone protective cap mold into the silicone impregnation liquid, with an immersion speed of 5-20 mm / s and an immersion time of 5-50 s; the rising speed after the immersion is 1-20 mm / s; placing the impregnated mold at 300-400°C for curing for 25-120 s, cooling to room temperature, and demolding to obtain the optical fiber array silicone protective cap.

[0021] Beneficial effects: The present invention designs a formula for a silicone impregnating liquid, and prepares a silicone protective cap for an optical fiber array for protecting a FA optical fiber connector based on the silicone impregnating liquid. It is verified through experimental data that the optical fiber array silicone protective cap prepared by the present invention performs well in physical properties such as hardness, tensile strength, tear strength and elongation at break, and there is no adhesion or debonding after 10 high and low temperature cycles, and the cap can be effectively used for the processing and protection of FA optical fiber connector products. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of a method for preparing a silicone protective cap for an optical fiber array.

[0023] Figure 2 Actual images of 5 groups of FA inserts selected from 10 groups of samples in Example 1 after high and low temperature cycles at 20 times the detection angle. DETAILED DESCRIPTION

[0024] The present invention provides a silicone protective cap for an optical fiber array and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0025] The terms "first", "second", "third", "fourth", etc. (if any) in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" or "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0026] The present invention provides a silicone protective cap for an optical fiber array. The silicone protective cap for the optical fiber array is formed by impregnating a silicone impregnation liquid on a mold and curing the impregnation liquid. The silicone impregnation liquid comprises, by weight: 50-250 parts of vinyl silicone oil, 10-40 parts of white carbon black, 1-5 parts of a surface treatment agent, 1-5 parts of deionized water, 5-20 parts of silicone resin, 5-35 parts of hydrogen-containing silicone oil, 1-10 parts of a fluorine-containing filler, 0.1-3 parts of an inhibitor, and 0.05-0.6 parts of a catalyst.

[0027] In the present invention, the vinyl-terminated silicone oil refers to a silicone oil containing vinyl groups at both ends of the molecular chain. The molecular structure of this silicone oil has a specific end group structure. The vinyl groups are located at both ends of the chain and may be bridged by silicon oxide compounds, but remain linear or have a slight branched structure as a whole. Typical representatives include vinyl-terminated polydimethylsiloxane (Vi-PDMS) and vinyl-terminated polymethylvinylsiloxane (Vi-PMVS). These silicone oils have specific reactivity and physical properties due to the presence of vinyl groups at their ends. Polyvinyl silicone oil refers to silicone oil containing multiple vinyl groups in the molecule. These vinyl groups may be distributed at different positions of the silicone oil molecule to form a more complex structure. It is formed by addition reaction of linear or cyclic siloxane monomers containing Si-O bonds, and the number and distribution of vinyl groups can be adjusted as needed. The viscosity of vinyl-terminated silicone oil is related to the molecular weight. Mixing vinyl-terminated silicone oils of different viscosities can increase the molecular weight distribution width of vinyl-terminated silicone oil, which is conducive to the formation of crosslinking points and the control of crosslinking density, improve the fluidity of the impregnation solution during preparation, make it easy to process, and ensure the stability of the impregnation solution. In the present invention, the vinyl silicone oil is composed of a terminal vinyl silicone oil with a viscosity of 5000mPa·s, a terminal vinyl silicone oil with a viscosity of 500mPa·s and a polyvinyl silicone oil in a weight ratio of (50-120):(20-60):(10-30). In the present invention, if the high-viscosity terminal vinyl silicone oil of 5000mPa·s is added in excessive amounts, its overall viscosity is too large and it is easy to cause the base rubber to be difficult to disperse during kneading; if the low-viscosity terminal vinyl silicone oil of 500mPa·s is added in excessive amounts, the base rubber is not strong enough and is not easy to vulcanize and mold. The vinyl silicone oil prepared by the present invention can ensure that the fluidity of the impregnation liquid during preparation is improved, making it easy to process, and ensuring the stability of the impregnation liquid.

[0028] In the present invention, the specific surface area of ​​white carbon black is 150-300m 2 / g. The hardness and tensile strength of silica gel increase with the increase of the specific surface area of ​​silica, while its fracture strength decreases with the increase of the specific surface area of ​​silica. Based on this, the present invention selects silica gel with a specific surface area of ​​150-300m 2 / g range of white carbon black, the resulting silicone rubber has the most appropriate softness and strength.

[0029] In the present invention, the white carbon black can be one or more of fumed white carbon black, precipitated white carbon black, and surface treated white carbon black, but is not limited thereto. The type, treatment method, and addition steps of white carbon black have a certain influence on its dispersion in the impregnation liquid. If the white carbon black is not evenly dispersed, the structure is serious, which will lead to an increase in the viscosity of the impregnation liquid and poor stability.

[0030] In the present invention, the hydrogen-containing silicone oil is at least one of terminal hydrogen-containing silicone oil and silicone oil containing active hydrogen in both the terminal group and the side chain, but is not limited thereto. The hydrogen-containing silicone oil plays a role in diluting the base rubber and cross-linking. The use of hydrogen-containing silicone oils of different types and hydrogen contents is conducive to adjusting the density between cross-linking points, increasing the fluidity of the impregnation liquid, and ensuring processing stability.

[0031] In the present invention, the silicone resin is one or more of methyl silicone resin, low phenyl methyl silicone resin, fluorosilicone resin, methyl MQ silicone resin and vinyl MQ silicone resin, but is not limited thereto.

[0032] In the present invention, the surface treatment agent is one or more of a silane coupling agent, a siloxane coupling agent and a silazane coupling agent, but is not limited thereto.

[0033] In the present invention, the fluorine-containing filler can be one or more of fluorine-containing nanomaterials, fluorine plastics and fluorine rubber, but is not limited thereto. Since the fluorine-containing filler has strong chemical inertness and low surface energy, low adhesion, non-stickiness, low friction, waterproofness and corrosion resistance, it can prevent the leaching of possible pollutants, reduce the direct contact surface between the FA optical fiber connector and the silica gel, and play a barrier role.

[0034] In the present invention, the inhibitor is one or more of acetylenic alcohol compounds, polyvinyl polysiloxane and maleate compounds, but not limited thereto; the catalyst is at least one of platinum-vinyl siloxane complex and alcohol-modified chloroplatinic acid complex, but not limited thereto. The inhibitor and catalyst are mainly used to adjust the molecular chain vulcanization and crosslinking rate. The above types and proportions of inhibitors and catalysts can be used to appropriately extend the processing operation time of the silicone impregnation solution and reduce costs.

[0035] The present invention designs a formula of silicone impregnation liquid, and prepares a fiber array silicone protective cap for protecting FA fiber optic connectors based on the silicone impregnation liquid. It is found through experimental data verification that the optical fiber array silicone protective cap prepared by the present invention has better performance in physical properties such as hardness, tensile strength, tear strength and elongation at break, and no adhesion or debonding occurs during 10 high and low temperature cycles. The optical fiber array silicone protective cap can be effectively used for the processing and protection of FA fiber optic connector products.

[0036] In some embodiments, a method for preparing the optical fiber array silicone protective cap according to the present invention is also provided, such as Figure 1 As shown, it includes the steps of:

[0037] S100, according to the proportion, put part of the terminal vinyl silicone oil with a viscosity of 5000mPa·s into the kneader, add half of the amount of white carbon black in batches, and knead at room temperature for 0.5-2h; continue kneading and add the remaining white carbon black, surface treatment agent and deionized water in batches during this process, and the kneader speed is 5-20 rpm; add the remaining total terminal vinyl silicone oil with a viscosity of 5000mPa·s and fluorine-containing filler, then heat to 80-150°C, and knead for 2-4h; finally evacuate, knead for 1-2h at a vacuum degree of 0.1-0.3MPa and a temperature of 120-150°C; add the terminal vinyl silicone oil and polyvinyl silicone oil with a viscosity of 500mPa·s in batches, knead for 1-3h, and the kneader speed is 10-30 rpm. After the stirring is completed, cool to room temperature, take out the rubber material and grind it to obtain a grinding product;

[0038] S200, putting the ground product into a planetary mixer, adding hydrogenated silicone oil in batches and stirring for 1-2 hours, adding an inhibitor and stirring for 0.5-2 hours, and finally adding a catalyst and stirring for 0.5-2 hours, with the mixer rotating at a speed of 50-80 rpm until the paste is evenly dispersed; after the stirring is completed, filtering with a sieve and degassing to obtain a silica gel impregnation solution;

[0039] S300, preheating the optical fiber array silicone protective cap mold at 200-370°C for 30-100s;

[0040] S400, immersing the preheated optical fiber array silicone protective cap mold into the silicone impregnation liquid, with an immersion speed of 5-20 mm / s and an immersion time of 5-50 s; the rising speed after the immersion is 1-20 mm / s; placing the impregnated mold at 300-400°C for curing for 25-120 s, cooling to room temperature, and demolding to obtain the optical fiber array silicone protective cap.

[0041] The present invention provides a method for preparing a silicone protective cap for an optical fiber array. The method is simple to operate and easy to implement. The optical fiber array silicone protective cap prepared by the present invention has better physical properties such as hardness, tensile strength, tear strength and elongation at break, and no adhesion or debonding occurs during 10 high and low temperature cycles. The silicone protective cap can be effectively used for the processing and protection of FA optical fiber connector products.

[0042] The present invention will be further explained below by means of specific embodiments:

[0043] Example 1

[0044] A method for preparing a silicone protective cap for an optical fiber array comprises the following steps:

[0045] 1. According to the proportion, half of the end-vinyl silicone oil with a viscosity of 5000mPa·s is put into the kneader, and half of the white carbon black is added in batches, and kneaded at room temperature for 1h; continue kneading and add the remaining white carbon black, surface treatment agent and deionized water in batches during this process, and the kneader speed is 10 rpm; add the remaining total end-vinyl silicone oil with a viscosity of 5000mPa·s and fluorine-containing filler, then heat to 120°C and knead for 3h; finally, evacuate, knead for 1.5h at a vacuum degree of 0.2MPa and a temperature of 140°C; add end-vinyl silicone oil and polyvinyl silicone oil with a viscosity of 500mPa·s in batches, knead for 2h, and the kneader speed is 20 rpm. After stirring, cool to room temperature, take out the rubber and grind it to obtain a grinding product;

[0046] 2. Put the ground product into a planetary mixer, add hydrogenated silicone oil in batches and stir for 1.5 hours, add inhibitor and stir for 1 hour, and finally add catalyst and stir for 1 hour, with the mixer rotating at 65 rpm until the paste is evenly dispersed; after stirring, filter with a sieve and deaerate to obtain a silica gel impregnation liquid, which comprises, by weight: 100 parts of vinyl silicone oil, 25 parts of white carbon black, 3 parts of a surface treatment agent, 3 parts of deionized water, 10 parts of silicone resin, 20 parts of hydrogenated silicone oil, 5 parts of fluorine-containing filler, 1.5 parts of inhibitor, and 0.3 parts of a catalyst. In this embodiment, the vinyl silicone oil is composed of 50 parts of terminal vinyl silicone oil with a viscosity of 5000 mPa·s, 30 parts of terminal vinyl silicone oil with a viscosity of 500 mPa·s, and 20 parts of polyvinyl silicone oil; white carbon black is a silica gel with a specific surface area of ​​200 m 2 / g of fumed silica; the silicone resin is composed of 5 parts of methyl silicone resin and 5 parts of fluorosilicone resin; the hydrogen-containing silicone oil is a terminal hydrogen-containing silicone oil; the surface treatment agent is a silane coupling agent; the fluorine-containing filler is a fluoroplastic; the inhibitor is polyvinyl polysiloxane; and the catalyst is a platinum-vinyl siloxane complex.

[0047] 3. Preheat the optical fiber array silicone protective cap mold at 300°C for 60 seconds;

[0048] 4. Immerse the preheated optical fiber array silicone protective cap mold into the silicone impregnation liquid at a dipping speed of 10 mm / s and a dipping time of 25 s; the rising speed after the dipping is 10 mm / s; place the impregnated mold at 350°C for 70 s, cool to room temperature, and demold to obtain the optical fiber array silicone protective cap.

[0049] Example 2

[0050] A method for preparing a silicone protective cap for an optical fiber array comprises the following steps:

[0051] 1. According to the ratio, put one-third of the terminal vinyl silicone oil with a viscosity of 5000mPa·s into the kneader, add half of the white carbon black in batches, and knead at room temperature for 2h; continue kneading and add the remaining white carbon black, surface treatment agent and deionized water in batches during this process, and the kneader speed is 20 rpm; add the remaining terminal vinyl silicone oil with a viscosity of 5000mPa·s and fluorine-containing filler, then heat to 150℃, and knead for 2h; finally evacuate, knead for 1h at a vacuum degree of 0.3MPa and a temperature of 120℃; add the terminal vinyl silicone oil and polyvinyl silicone oil with a viscosity of 500mPa·s in batches, knead for 3h, and the kneader speed is 10 rpm. After stirring, cool to room temperature, take out the rubber and grind it to obtain a grinding product;

[0052] 2. Put the ground product into a planetary mixer, add hydrogenated silicone oil in batches and stir for 2 hours, add inhibitor and stir for 0.5 hours, and finally add catalyst and stir for 2 hours, with the mixer rotating at 50 rpm until the paste is evenly dispersed; after stirring, filter with a sieve and deaerate to obtain a silica gel impregnation liquid, which comprises, by weight: 200 parts of vinyl silicone oil, 40 parts of white carbon black, 5 parts of a surface treatment agent, 5 parts of deionized water, 20 parts of silicone resin, 30 parts of hydrogenated silicone oil, 10 parts of a fluorine-containing filler, 3 parts of an inhibitor, and 0.6 parts of a catalyst; in this embodiment, the vinyl silicone oil is composed of 120 parts of a terminal vinyl silicone oil with a viscosity of 5000 mPa·s, 50 parts of a terminal vinyl silicone oil with a viscosity of 500 mPa·s, and 30 parts of a polyvinyl silicone oil; the white carbon black is a silica with a specific surface area of ​​300 m 2 / g of precipitated silica; the silicone resin is composed of 15 parts of methyl silicone resin and 5 parts of methyl MQ silicone resin; the hydrogen-containing silicone oil is silicone oil containing active hydrogen in both the end group and the side chain; the surface treatment agent is a siloxane coupling agent; the fluorine-containing filler is fluororubber; the inhibitor is an acetylenic alcohol compound; and the catalyst is an alcohol-modified chloroplatinic acid complex.

[0053] 3. Preheat the optical fiber array silicone protective cap mold at 350°C for 100 seconds;

[0054] 4. Immerse the preheated optical fiber array silicone protective cap mold into the silicone impregnation liquid at a dipping speed of 20 mm / s and a dipping time of 5 s; the rising speed after dipping is 20 mm / s; place the impregnated mold at 400°C for 25 s, cool to room temperature, and demold to obtain the optical fiber array silicone protective cap.

[0055] Example 3

[0056] A method for preparing a silicone protective cap for an optical fiber array comprises the following steps:

[0057] 1. According to the proportion, half of the terminal vinyl silicone oil with a viscosity of 5000mPa·s is put into the kneader, and half of the amount of white carbon black is added in batches, and kneaded at room temperature for 0.5h; continue kneading and add the remaining white carbon black, surface treatment agent and deionized water in batches during this process, and the kneader speed is 20 rpm; add the remaining total terminal vinyl silicone oil with a viscosity of 5000mPa·s and fluorine-containing filler, then heat to 80°C and knead for 4h; finally evacuate, knead for 2h at a vacuum degree of 0.1MPa and a temperature of 150°C; add the terminal vinyl silicone oil and polyvinyl silicone oil with a viscosity of 500mPa·s in batches, knead for 1h, and the kneader speed is 30 rpm. After stirring, cool to room temperature, take out the rubber and grind it to obtain a grinding product;

[0058] 2. Put the ground product into a planetary mixer, add hydrogenated silicone oil in batches and stir for 1 hour, add inhibitor and stir for 2 hours, and finally add catalyst and stir for 0.5 hour, and the mixer speed is 80 rpm until the paste is evenly dispersed; after the stirring is completed, filter with a sieve and deaerate to obtain a silica gel impregnation liquid, which comprises, by weight: 50 parts of vinyl silicone oil, 10 parts of white carbon black, 1 part of a surface treatment agent, 2 parts of deionized water, 5 parts of silicone resin, 5 parts of hydrogenated silicone oil, 1 part of a fluorine-containing filler, 0.1 parts of an inhibitor, and 0.1 parts of a catalyst; in this embodiment, the vinyl silicone oil is composed of 25 parts of terminal vinyl silicone oil with a viscosity of 5000 mPa·s, 15 parts of terminal vinyl silicone oil with a viscosity of 500 mPa·s, and 10 parts of polyvinyl silicone oil; the white carbon black is a silica with a specific surface area of ​​150 m 2 / g of precipitated silica; the silicone resin is composed of 2 parts of methyl silicone resin and 3 parts of methyl MQ silicone resin; the hydrogen-containing silicone oil is silicone oil containing active hydrogen in both the end group and the side chain; the surface treatment agent is a siloxane coupling agent; the fluorine-containing filler is fluororubber; the inhibitor is an acetylenic alcohol compound; and the catalyst is an alcohol-modified chloroplatinic acid complex.

[0059] 3. Preheat the optical fiber array silicone protective cap mold at 200°C for 100 seconds;

[0060] 4. Immerse the preheated optical fiber array silicone protective cap mold into the silicone impregnation liquid at a dipping speed of 5 mm / s and a dipping time of 50 s; the rising speed after dipping is 1 mm / s; place the impregnated mold at 400°C for curing for 25 s, cool to room temperature, and demold to obtain the optical fiber array silicone protective cap.

[0061] Example 4

[0062] A method for preparing a silicone protective cap for an optical fiber array comprises the following steps:

[0063] 1. According to the ratio, put one-fourth of the terminal vinyl silicone oil with a viscosity of 5000mPa·s into the kneader, add half of the white carbon black in batches, and knead at room temperature for 1h; continue kneading and add the remaining white carbon black, surface treatment agent and deionized water in batches during this process, and the kneader speed is 15 rpm; add the remaining total terminal vinyl silicone oil with a viscosity of 5000mPa·s and fluorine-containing filler, then heat to 100°C and knead for 2h; finally evacuate, knead for 1h at a vacuum degree of 0.1MPa and a temperature of 130°C; add terminal vinyl silicone oil and polyvinyl silicone oil with a viscosity of 500mPa·s in batches, knead for 1h, and the kneader speed is 30 rpm. After stirring, cool to room temperature, take out the rubber and grind it to obtain a grinding product;

[0064] 2. Put the ground product into a planetary mixer, add hydrogenated silicone oil in batches and stir for 2 hours, add inhibitor and stir for 2 hours, and finally add catalyst and stir for 2 hours, the mixer speed is 80 rpm until the paste is evenly dispersed; after the stirring is completed, filter with a sieve and deaerate to obtain a silica gel impregnation liquid, which comprises, by weight: 80 parts of vinyl silicone oil, 15 parts of white carbon black, 2 parts of a surface treatment agent, 3 parts of deionized water, 12 parts of silicone resin, 20 parts of hydrogenated silicone oil, 4 parts of fluorine-containing filler, 1 part of inhibitor, and 0.2 parts of catalyst; in this embodiment, the vinyl silicone oil is composed of 50 parts of terminal vinyl silicone oil with a viscosity of 5000 mPa·s, 20 parts of terminal vinyl silicone oil with a viscosity of 500 mPa·s and 10 parts of polyvinyl silicone oil; the white carbon black is a silica gel with a specific surface area of ​​250 m 2 / g of fumed silica; the silicone resin is composed of 6 parts of methyl silicone resin and 6 parts of fluorosilicone resin; the hydrogen-containing silicone oil is a terminal hydrogen-containing silicone oil; the surface treatment agent is a silazane coupling agent; the fluorine-containing filler is a fluorine-containing nanomaterial; the inhibitor is polyvinyl polysiloxane; and the catalyst is a platinum-vinyl siloxane complex.

[0065] 3. Preheat the optical fiber array silicone protective cap mold at 220°C for 50 seconds;

[0066] 4. Immerse the preheated optical fiber array silicone protective cap mold into the silicone impregnation liquid at a dipping speed of 8 mm / s and a dipping time of 20 s; the rising speed after dipping is 4 mm / s; place the impregnated mold at 340°C for curing for 100 s, cool to room temperature, and demold to obtain the optical fiber array silicone protective cap.

[0067] Test Example 1

[0068] The optical fiber array silicone protective caps prepared in Examples 1-4 were subjected to performance tests of hardness, elongation at break, tensile strength and tear strength, wherein hardness test: GB / T 2411-2008 Plastics and hard rubber, using a hardness tester to measure indentation hardness (Shore hardness); elongation at break and tensile strength: GB / T 1040.3-2006 Determination of tensile properties of plastics Part 3: Test conditions for films and sheets; tear strength: GB / T 529-2008 Determination of tear strength of vulcanized rubber or thermoplastic rubber (trouser-shaped, right-angled and crescent-shaped specimens); the test results are shown in Table 1:

[0069] Table 1 Test results

[0070] Hardness(HA) Tensile strength(MPa) Tear strength(N / mm) Elongation at break (%) Example 1 36 5 12 330 Example 2 35 4 12 320 Example 3 35 3 10 305 Example 4 30 3 7 235

[0071] Test Example 2

[0072] The 10 groups of sample optical fiber array silicone protective caps prepared in Example 1 were put on the FA ferrule, and the FA ferrule was UV glued and cured by UV light. Then, the samples were subjected to 85°C / 15min and -40°C / 15min high and low temperature cycles for 10 times. After the cycle, the optical fiber array silicone protective caps were removed to detect whether the optical fiber array silicone protective caps had adhesion and debonding problems on the FA ferrule. The results are as follows: Figure 2 As shown in Table 2, Figure 2 The actual picture of the FA ferrule at 20 times detection after the silicone protective caps of the optical fiber arrays of 5 groups of samples randomly selected from the 10 groups of samples were put on the FA ferrule and subjected to 10 high and low temperature cycles.

[0073] Table 2 Adhesion of each group after high and low temperature cycle

[0074]

[0075]

[0076] From Table 1-2 and Figure 2 The results show that the optical fiber array silicone protective cap prepared in the embodiment of the present invention performs well in physical properties such as hardness, tensile strength, tear strength and elongation at break, and there is no adhesion or debonding after 10 high and low temperature cycles, and it can be effectively used in the processing and protection of FA optical fiber connector products.

[0077] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A silicone protective cap for an optical fiber array, characterized in that: The optical fiber array silicone protective cap is formed by impregnating a silicone impregnation liquid on a mold and curing it. The silicone impregnation liquid includes, by weight: 50-250 parts of vinyl silicone oil, 10-40 parts of white carbon black, 1-5 parts of a surface treatment agent, 1-5 parts of deionized water, 5-20 parts of silicone resin, 5-35 parts of hydrogen-containing silicone oil, 1-10 parts of fluorine-containing filler, 0.1-3 parts of an inhibitor, and 0.05-0.6 parts of a catalyst.

2. The optical fiber array silicone protective cap according to claim 1, characterized in that: The vinyl silicone oil is composed of a mixture of vinyl-terminated silicone oil with a viscosity of 5000 mPa·s, vinyl-terminated silicone oil with a viscosity of 500 mPa·s and polyvinyl silicone oil in a weight ratio of (50-120):(20-60):(10-30).

3. The optical fiber array silicone protective cap according to claim 1, characterized in that: The surface treatment agent is one or more of a silane coupling agent, a siloxane coupling agent and a silazane coupling agent.

4. The optical fiber array silicone protective cap according to claim 1, characterized in that: The silicone resin is one or more of methyl silicone resin, low phenyl methyl silicone resin, fluorosilicone resin, methyl MQ silicone resin and vinyl MQ silicone resin.

5. The optical fiber array silicone protective cap according to claim 1, characterized in that: The fluorine-containing filler is one or more of fluorine-containing nanomaterials, fluorine plastics and fluorine rubber.

6. The optical fiber array silicone protective cap according to claim 1, characterized in that: The hydrogen-containing silicone oil is at least one of a terminal hydrogen-containing silicone oil and a silicone oil containing active hydrogen in both the terminal group and the side chain.

7. The optical fiber array silicone protective cap according to claim 1, characterized in that: The inhibitor is one or more of acetylenic alcohol compounds, polyvinyl polysiloxane and maleate compounds.

8. The optical fiber array silicone protective cap according to claim 1, characterized in that: The catalyst is at least one of a platinum-vinylsiloxane complex and an alcohol-modified chloroplatinic acid complex.

9. The optical fiber array silicone protective cap according to claim 1, characterized in that: The specific surface area of ​​the white carbon black is 150-300m 2 / g.

10. A method for preparing a silicone protective cap for an optical fiber array as claimed in any one of claims 1 to 9, characterized in that: Includes steps: According to the proportion, part of the terminal vinyl silicone oil with a viscosity of 5000mPa·s is put into the kneader, half of the amount of white carbon black is added in batches, and kneading is carried out at room temperature for 0.5-2h; kneading is continued and the remaining white carbon black, surface treatment agent and deionized water are added in batches during the process, and the kneader speed is 5-20 rpm; the remaining total terminal vinyl silicone oil with a viscosity of 5000mPa·s and fluorine-containing filler are added, and then the temperature is raised to 80-150°C and kneading is carried out for 2-4h; finally, vacuuming is carried out, and kneading is carried out for 1-2h at a vacuum degree of 0.1-0.3MPa and a temperature of 120-150°C; terminal vinyl silicone oil and polyvinyl silicone oil with a viscosity of 500mPa·s are added in batches, and kneading is carried out for 1-3h, and the kneader speed is 10-30 rpm. After the stirring is completed, it is cooled to room temperature, and the rubber material is taken out and ground to obtain a ground product; The ground product is put into a planetary mixer, hydrogenated silicone oil is added in batches and stirred for 1-2 hours, an inhibitor is added and stirred for 0.5-2 hours, and finally a catalyst is added and stirred for 0.5-2 hours, and the mixer speed is 50-80 rpm until the paste is evenly dispersed; after the stirring is completed, the silica gel impregnation liquid is obtained by filtering with a sieve and degassing. Preheat the optical fiber array silicone protective cap mold at 200-370°C for 30-100 seconds; The preheated optical fiber array silicone protective cap mold is immersed in the silicone impregnation liquid, with an impregnation speed of 5-20 mm / s and an impregnation time of 5-50 s; the rising speed after the impregnation is 1-20 mm / s; the impregnated mold is placed at 300-400° C. for curing for 25-120 s, cooled to room temperature, and demolded to obtain the optical fiber array silicone protective cap.