Method for producing ceramic coating

The integration of slow-release particles with silicone oil in ceramic coatings addresses the short lifespan issue, providing a long-lasting non-stick solution by controlling silicone oil release.

CN119060569AActive Publication Date: 2024-12-03WUHAN SUPOR COOKWARE +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310649792.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Ceramic coatings exhibit short non-stick lifespan, making them less desirable than PTFE products and unable to meet consumer demands for long-lasting non-stick utensils, especially under high-temperature cooking conditions and wear and tear.

Method used

A ceramic coating method incorporating slow-release particles with a disordered porous and/or layered structure, combined with silicone oil, is used to form a non-stick layer that slows down silicone oil release during cooking, maintaining long-lasting non-stick properties.

Benefits of technology

The method enhances the non-stick performance of ceramic coatings by prolonging the non-stick effect through controlled silicone oil release, significantly improving durability and longevity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060569A_ABST
    Figure CN119060569A_ABST
Patent Text Reader

Abstract

There is provided a method of making a ceramic coating, the method comprising: preparing a ceramic coating; and forming the ceramic coating on a substrate using a process of forming a layer, in which the method of preparing the ceramic coating comprises: preparing a ceramic coating precursor; preparing sustained-release particles; and mixing the ceramic coating precursor with the sustained release particles to obtain the ceramic coating. The sustained-release particles comprise a sustained-release material and silicone oil combined with the sustained-release material. The slow-release material comprises at least one of vermiculite, zeolite, bentonite, diatomite, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing a ceramic coating. Background Art

[0002] Currently, non-stick technologies mainly include PTFE coatings and ceramic coatings. Ceramic coatings are very limited in use due to their short non-stick lifespan. They are far less widely used than PTFE products and cannot meet consumers' daily demand for non-stick utensils. For example, non-stick pans will stick to the pan after about one month of use in an average household, especially in high-temperature cooking methods such as Chinese cooking, and under the condition of wear and tear of metal spatulas, the non-stick properties decay very quickly.

[0003] Therefore, improving the long-lasting non-stick properties of ceramic coatings has become a very meaningful and urgent technical need. Summary of the invention

[0004] Based on the above-mentioned deficiencies of the prior art, the present invention provides a method for forming a ceramic coating using a ceramic coating including slow-release particles.

[0005] According to one aspect of an exemplary embodiment, a method for manufacturing a ceramic coating includes: preparing a ceramic coating precursor and slow-release particles separately and mixing them to prepare a ceramic coating; and forming the ceramic coating on a substrate using a layer-forming process using the ceramic coating. The slow-release particles include a slow-release material and silicone oil bound to the slow-release material, wherein the slow-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate, and layered sulfate.

[0006] The steps of preparing a ceramic coating precursor may include:

[0007] S1: providing material A, material B and material C, wherein: material A comprises a silane substance; material B comprises silica sol and filler as essential components, optional pigment, wetting agent, thickener and emulsifier as unnecessary components, and solvent; material C comprises an organic acid as an essential component, and optional pH buffer and catalyst as unnecessary components;

[0008] S2: mixing material B and material C, and adjusting the pH of the mixture to acidic, thereby obtaining a first material;

[0009] S3: Mixing the A material with the first material to obtain a ceramic coating precursor.

[0010] According to another aspect of the exemplary embodiment, a method for manufacturing a ceramic coating includes: preparing a ceramic coating; and using the ceramic coating to form the ceramic coating on a substrate using a layer forming process, wherein the step of preparing the ceramic coating includes: preparing a material A including a silane substance, a material B including a silica sol and a filler, a material C including an organic acid, and slow-release particles; mixing the material B with the material C, and adjusting the pH of the mixture to acidic, thereby obtaining a first material; the first material is mixed with the material A and the slow-release particles, and the ceramic coating is obtained after the mixture reacts. The slow-release particles include a slow-release material and silicone oil bound to the slow-release material, wherein the slow-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate, and layered sulfate.

[0011] The particle size of the sustained-release particles may be less than or equal to 20 microns.

[0012] The step of preparing the sustained-release granules may include: providing a sustained-release material and silicone oil; mixing 35-58 parts by weight of the sustained-release material with 42-60 parts by weight of the silicone oil so that the silicone oil is combined with the sustained-release material to obtain the sustained-release granules.

[0013] The step of preparing the sustained-release particles may further include: controlling the particle size of the sustained-release particles to be less than or equal to 20 microns by a grinding process.

[0014] In the step of preparing sustained-release particles, silicone oil can be evenly mixed with a sustained-release material with a particle size of 100 mesh-3000 mesh and ground to a particle size less than or equal to 30 microns, and then a catalyst is added and ground to a particle size less than or equal to 20 microns to obtain sustained-release particles with a particle size less than or equal to 20 microns.

[0015] After grinding, the resultant may be treated with ultrasonic waves.

[0016] In terms of weight percentage, the silicone oil may include 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil, wherein the molecular weight of the low molecular weight silicone oil may be between 500-1000, the molecular weight of the medium molecular weight silicone oil may be between 3000-6000, and the molecular weight of the high molecular weight silicone oil may be between 12000-30000.

[0017] The slow-release particles may be included in an amount of 5.15-32.79 parts by weight per 100 parts by weight of the ceramic coating.

[0018] The silane material may include at least one of methyltrimethoxysilane, methyltriethoxysilane, and dimethyldimethoxysilane.

[0019] The A material may further include tetraethyl orthosilicate, and in the A material, the silane substance accounts for 80%-97% by weight, and the tetraethyl orthosilicate accounts for 3%-20% by weight. The ceramic coating may include at least one layer.

[0020] The ceramic coating may have a thickness of 10 micrometers to 80 micrometers.

[0021] The present invention provides that by adding slow-release particles including slow-release materials to a ceramic coating, a disordered porous and / or layered structure can be formed, in which case silicone oil can be bound to the slow-release material. Therefore, during the cooking process, due to the porous and / or layered structure of the slow-release material, the release of silicone oil can be slowed down, thereby maintaining a long-lasting non-stick effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a schematic diagram showing a ceramic coating according to an exemplary embodiment;

[0023] Figure 2 is a schematic enlarged view showing sustained-release particles in a ceramic coating according to an exemplary embodiment. DETAILED DESCRIPTION

[0024] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which embodiments are shown. However, the present invention may be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that the disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. The same reference numerals refer to the same elements throughout.

[0025] Ceramic coatings achieve non-stick properties mainly through the use of silicone methyl and doped silicone oil in the ceramic coating. As the product is heated and worn during use, the silicone oil in the coating will gradually be lost, destroying the silicone methyl groups on the surface, resulting in the loss of the non-stick effect, and finally the phenomenon of sticking to the pan when cooking. If the ceramic coating can store oil continuously, it can form an effective oil film to isolate the food and the coating surface, thereby achieving long-lasting non-stick properties.

[0026] Therefore, the present invention provides a ceramic coating, in which slow-release particles containing a slow-release material are included, and the slow-release material can have a disordered porous and / or layered structure, and silicone oil is combined (e.g., adsorbed, bonded) to the slow-release material. During the cooking process, the release of silicone oil is slowed down, thereby maintaining a long-lasting non-stick effect. However, the exemplary embodiments are not limited to this, and those skilled in the art can apply the ceramic coating to any prior art suitable for non-stick (such as non-stick coatings of cooking pots (e.g., frying spoons, rice cooker pots), inner and outer coatings of transport pipelines, etc.) based on the concept of the present invention.

[0027] Figure 1 is a schematic diagram showing an embodiment of a ceramic coating according to an exemplary embodiment, Figure 2 is a schematic diagram showing a slow-release particle in a ceramic coating according to an exemplary embodiment. Figure 1 and Figure 2 The method of manufacturing a ceramic coating according to the present invention will be described.

[0028] The method of manufacturing a ceramic coating according to the inventive concept may include: providing a substrate 100 and a ceramic coating; and forming a ceramic coating 200 on the substrate 100 using the ceramic coating using a layer forming process.

[0029] According to an exemplary embodiment, the substrate 100 may be a substrate known in the art for making cookware, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, etc. However, the present invention does not limit the material, use, and other properties of the substrate, that is, those skilled in the art may use any material on which a ceramic coating is to be applied as the substrate 100 as needed.

[0030] Before, during or after providing the substrate 100, a ceramic coating may be prepared. According to an exemplary embodiment, the ceramic coating may include a ceramic coating precursor 1 and slow-release particles 2 dispersed in the ceramic coating precursor. Therefore, the step of providing the ceramic coating may include the steps of preparing the ceramic coating precursor 1 and the slow-release particles 2, respectively, and mixing the ceramic coating precursor 1 with the slow-release particles 2 to obtain the ceramic coating. Here, the ceramic coating precursor 1 may be equivalent to the ceramic coating used in the art, and therefore, may have the components of the ceramic coating conventionally used in the art, so that the method for preparing the ceramic coating known in the art may be used. However, the exemplary embodiment is not limited thereto, as mentioned in the method for manufacturing the ceramic coating precursor 1 according to the inventive concept described below in conjunction with the exemplary embodiment, the ceramic coating precursor 1 may be prepared by the method described below, or those skilled in the art may also combine the step of preparing the ceramic coating precursor 1 with the step of preparing the slow-release particles, and the ceramic coating precursor 1 prepared by the method of the inventive concept to be described below may have a more excellent feature of cooperating with the slow-release particles to provide non-stickiness. The method for manufacturing the ceramic coating of the related art will not be redundantly described here, and a method for preparing the ceramic coating according to the present inventive concept by separately preparing a ceramic coating precursor and slow-release particles will be mainly described.

[0031] Preparation of ceramic coating precursors

[0032] According to an exemplary embodiment, the step of preparing the ceramic coating precursor may include a step of providing materials and a step of mixing.

[0033] The step of providing materials may include the steps of separately providing A material, B material and C material.

[0034] Here, material A may include a silane substance, material B may include silica sol and filler as essential components, optional pigments, wetting agents, thickeners and emulsifiers as unnecessary components and a solvent, and material C may include an organic acid as an essential component, and optional pH buffers and catalysts (e.g., zirconium acetate) as unnecessary components.

[0035] In the A material, according to an exemplary embodiment, the silane substance is used to form polysiloxane during the formation of the ceramic coating, and therefore, the silane substance here may include a substance known in the art for polycondensation to form polysiloxane. According to an exemplary embodiment, the silane substance may include at least one of methyltrimethoxysilane, methyltriethoxysilane, and dimethyldimethoxysilane, but is not limited thereto. In addition, in addition to the silane substance, the A material may also include tetraethyl orthosilicate that is polycondensed to form polysiloxane, and in this case, in the A material, by weight percentage, the silane substance may account for 80%-97% of the A material, and the tetraethyl orthosilicate may account for 3%-20% of the A material.

[0036] Material B may necessarily include fillers and silica sol. The filler plays a role in increasing the wear resistance of the coating, etc. Therefore, the present invention does not limit the type of filler, and ordinary commonly used fillers can be selected, for example, at least one of mica powder, kaolin, montmorillonite, silicon carbide, alumina and silicon dioxide can be selected. In addition, silica sol is the main film-forming substance of ceramic coatings, which reacts with polysiloxane under acidic conditions to form a ceramic coating. Therefore, commercially available ordinary silica sol can be selected as the silica sol in material B of the present invention. For example, the silica sol can be Akzo Nobel 1050 (silica sol) or American Grace LUDIXAM-50.

[0037] The necessary components in the B material can be dispersed in a solvent. That is, the B material can also include a solvent. Here, the solvent can include deionized water, and in order to adjust the volatilization rate of the solvent during the coating drying process, the solvent can also include isopropanol. In addition, the ratio between isopropanol and water is unlimited, and the ratio between water and isopropanol can be selectively proportioned according to actual needs.

[0038] In the B material, in addition to the above-mentioned necessary components, one or more of a pigment, a wetting agent, a thickener and an emulsifier may be selectively included as an unnecessary component. Here, the pigment is mainly used to give the coating different colors, so ordinary inorganic pigments can be selected. Inorganic pigments have good temperature resistance and good safety, and inorganic pigments are preferably selected in the high temperature resistant field. According to an exemplary embodiment, at least one of carbon black, copper chrome black, titanium dioxide, iron oxide, etc. may be selected as a filler. In addition, during the preparation of the necessary components in the solvent, in order to provide the excellent properties of the material, at least one of a wetting agent, a thickener and an emulsifier may also be added to the material.

[0039] According to a specific example, the B material may include, by weight percent: 30wt%-48wt% of silica sol, 8wt%-13wt% of pigment, 8wt%-25wt% of filler, 0.2wt%-1wt% of wetting agent, 1wt%-3wt% of thickener, 3wt%-5wt% of emulsifier, and the balance is isopropyl alcohol and deionized water. However, exemplary embodiments are not limited thereto, and one or more of the unnecessary components may be omitted.

[0040] The C material is used as a strong acid catalyst, and may include an organic acid as an essential component, and an optional pH buffer and a catalyst (e.g., zirconium acetate) as an unnecessary component. Here, the organic acid is used to adjust the pH value of the silica sol in the subsequent process so that it can react with the A material in an acidic environment, and therefore, an organic acid commonly used in the art for ceramic coatings can be used. According to an exemplary embodiment, at least one of formic acid and acetic acid can be selected as an organic acid, and when both formic acid and acetic acid are included, the weight ratio between formic acid and acetic acid can be between 4:6 and 1:1. In addition, in the C material, a pH buffer and a catalyst may also be selectively included. Here, the pH buffer and the catalyst may be a pH buffer and a catalyst used in the process of preparing a strong acid catalyst for ceramic coatings known in the art, for example, the pH buffer may be a weak acid such as boric acid, and the catalyst is used to accelerate the reaction rate of the sol-gel, and may be zirconium acetate, etc. However, the exemplary embodiment is not limited to the types of pH buffers and catalysts, and suitable pH buffers and catalysts may be omitted or appropriately selected based on the prior art.

[0041] According to an exemplary embodiment, the C material may include 80-97 parts by weight of a mixture of formic acid and acetic acid, 1-2 parts by weight of a boric acid pH buffer, and 0.5 parts by weight of a zirconium acetate catalyst.

[0042] After providing the above-mentioned materials, a mixing step may be performed. Herein, the mixing step may include a first mixing step of mixing the B material with the C material and a second step of mixing the result of the first mixing step (ie, the first material described below) with the A material.

[0043] Specifically, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidic (e.g., to less than or equal to 4) by utilizing the acidity of the C material to obtain the first material. Since the C material includes a solid filler and an optional pigment, the C material can be added to a grinder and ground for 0.5h-2h before mixing or during the preparation of the C material, so that it is fully dispersed and ground to a particle size of less than or equal to 15 microns to obtain a uniformly dispersed slurry.

[0044] After the B material and the C material are mixed, the mixture may be tumbling dispersed for a predetermined time (eg, 0.5 h) so that the first material has a high degree of dispersion.

[0045] After obtaining the first material, material A may be added to the first material. Here, the weight ratio of the added amount of material A to material B may be in the range of (20-30):(40-60). After adding material A, material A and material B may be shaken evenly so that material A and material B undergo a sol-gel reaction in an acidic environment to form a ceramic coating precursor.

[0046] Preparation of sustained-release granules

[0047] The slow-release particles can be prepared during, before, or after the preparation of the ceramic coating precursor. The slow-release particles can be prepared by mixing the slow-release material with silicone oil.

[0048] According to an exemplary embodiment, the sustained-release particle 2 may include a sustained-release material 21 having a pore structure and / or a layer structure and a silicone oil 22 combined with (eg, adsorbed, bonded to) the sustained-release material.

[0049] A slow-release material precursor of appropriate size (i.e., a slow-release material before grinding, when the grinding step is omitted, the slow-release material precursor can be considered as the slow-release material used in the end) can be selected to prepare slow-release particles. According to an exemplary embodiment, the slow-release material precursor can have a layer gap and / or pore structure. According to the example, the slow-release material precursor can include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material precursor has a porous and / or layered structure and the slow-release material formed after grinding is combined with silicone oil. The silicone oil combined with the slow-release material can be slowly released during the use of the cookware with a non-stick coating formed by the ceramic coating conceived by the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick layer formed by the ceramic coating.

[0050] According to an exemplary embodiment, the particle size of the slow-release material precursor may be in the range of 100 mesh to 3000 mesh (e.g., in the range of 100 mesh sieve to 3000 mesh sieve), and the particle size of the slow-release material within this range may obey a normal distribution. However, when the particle size is too large (e.g., on a 100 mesh sieve), the excessively large particle size is likely to increase the grinding process or make the particle size of the slow-release material after grinding too large, ultimately affecting the appearance of the non-stick coating made using the ceramic coating; on the contrary, the particle size is too small (e.g., under a 3000 mesh sieve, and the particle size will be smaller after grinding) It is not easy to effectively adsorb and bond silicone oil, and thus it is not easy to achieve a good silicone oil slow-release effect.

[0051] When the slow-release material precursor has the above-mentioned particle size distribution, the particle size of the slow-release material finally obtained can be made to be less than 20 microns by using two grinding processes as described below. However, the exemplary embodiment is not limited thereto, that is, when the slow-release material precursor is selected to have a smaller particle size value within the range of 100 mesh-3000 mesh, one grinding process can be omitted; in addition, when the particle size of the slow-release material precursor is selected to have a smaller particle size value within the above-mentioned range, two grinding processes can be omitted. When at least one of the grinding processes is omitted, the omitted grinding process can be replaced by a stirring process, or the mixture can be left untreated.

[0052] According to an exemplary embodiment, the silicone oil 22 is combined (e.g., adsorbed, bonded) with the sustained-release material 21 and provides the main non-stickiness for the ceramic coating. The silicone oil can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, and polyether modified silicone oil, and can be mixed by silicone oils of different molecular weights in a certain proportion to form a silicone oil composition with a molecular weight normal distribution; wherein, by weight percentage, the low molecular weight silicone oil content can be 20wt%-30wt%, the medium molecular weight silicone oil content can be 40wt%-60wt%, and the high molecular weight silicone oil content can be 20wt%-30wt%. Here, the molecular weight of the low molecular weight silicone oil can be between 500-1000, the molecular weight of the medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of the high molecular weight silicone oil can be between 12000-30000. By utilizing a normally distributed silicone oil composition, the sustained-release and non-stick effects can be better exerted. This is because: high molecular weight silicone oil is more firmly bonded to the sustained-release material and releases more slowly; low molecular weight silicone oil has better free mobility and thus better non-stick properties; in addition, medium molecular weight silicone oil takes into account both free mobility and strong bonding. Therefore, low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil can be combined to better exert the sustained-release and non-stick effects.

[0053] According to an example, 35-58 parts by weight of a slow-release material precursor can be mixed with 42-60 parts by weight of silicone oil to obtain a mixture, and 1 part by weight of a coupling agent (e.g., a methoxysilane coupling agent), 0.3 parts by weight of a catalyst (e.g., a titanate catalyst) and 1-1.5 parts by weight of a dispersant can be added to the mixture to prepare slow-release particles. Here, the coupling agent and the catalyst are used to enhance the bonding force between the silicone oil and the slow-release material, and the dispersant is used to improve the dispersion of the slow-release material in the silicone oil. Therefore, the exemplary embodiment is not limited to the case of including a coupling agent, a dispersant and a catalyst, and at least one of the coupling agent, the catalyst and the dispersant can be omitted.

[0054] According to a specific example, the silicone oil, the slow-release material precursor with a particle size of 100 mesh sieve-3000 mesh sieve and the silane coupling agent can be mixed uniformly according to the above ratio, and ground to a particle size of less than or equal to 30 microns, and then the catalyst is added, and the particle size is continued to be less than or equal to 20 microns, and then ultrasonic treatment is performed at room temperature (e.g., 22°C) for 0.5h-1h, so that the slow-release particles can be obtained. Here, firstly mixing the silicone oil with the slow-release material precursor and then grinding to a particle size of less than or equal to 30 microns can make the silicone oil and the slow-release material mixed uniformly, and then grinding to a particle size of less than or equal to 20 microns under the condition of the catalyst can make the silicone oil fully firmly adsorbed and bonded to the outside of the slow-release material. However, when the particle size of the slow-release material precursor is less than 30 microns, the first grinding can be omitted, and optionally a stirring process can be provided, or the second grinding process can be directly performed. In addition, when the particle size of the sustained-release material precursor is less than 15 μm, the second grinding process can be further omitted. At this time, the sustained-release material precursor is equivalent to the sustained-release material to be finally used, and a stirring process can be optionally provided.

[0055] Preparation of ceramic coatings

[0056] After the ceramic coating precursor and the slow-release particles are prepared, the slow-release particles may be mixed with the ceramic coating precursor to prepare a ceramic coating according to an exemplary embodiment.

[0057] According to an exemplary embodiment, during the preparation of the ceramic coating, based on the total weight of the ceramic coating, 61-92 parts by weight of a ceramic coating precursor can be mixed with 5-30 parts by weight of slow-release particles (for example, the weight ratio of A, B, C and slow-release particles D can be (20-30): (40-60): (1-2): (5-30)), and after the ceramic coating precursor and the slow-release particles are mixed, the mixture can be stirred at a speed of 120 rpm to 200 rpm for 6h to 8h to obtain the desired ceramic coating.

[0058] In addition, although the above describes a method of obtaining a ceramic coating by separately preparing a ceramic coating precursor and slow-release particles and mixing the ceramic coating precursor with the slow-release particles, in a method of combining the step of preparing a ceramic coating precursor with the step of preparing slow-release particles, as described above, after mixing the B material with the C material, the A material and the slow-release particles can be added to the mixture of the B material and the C material at the same time. For example, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidic (for example, less than or equal to 4) by using the acidity of the C material to obtain the first material. Then, the A material and the slow-release particles can be added to the mixture, where the weight ratio of the added amount of the A material, the slow-release particles and the B material can be in the range of (20-30): (5-30): (40-60). After mixing, the mixture can be stirred at a speed of 120-200 rpm for 6h-8h to obtain the desired ceramic coating.

[0059] Preparation of ceramic coating

[0060] After the ceramic paint is obtained, a ceramic coating layer may be formed on the substrate 100 using a layer forming process using the ceramic paint.

[0061] For example, the ceramic coating can be sprayed by air spraying. Here, the air spraying parameters are as follows: the spraying distance is 160 mm; the air pressure is 0.3 MPa; the flow rate is 8 L / min. However, the exemplary embodiment is not limited thereto, and those skilled in the art may use other layer-forming methods to form a ceramic coating using the ceramic coating conceived by the present invention. In addition, in order to improve the bonding force between the ceramic coating 200 and the substrate 100, the substrate may be treated. For example, the substrate may be sandblasted with 60# brown corundum to form a surface roughness of 3-6 microns, and then the substrate may be cleaned and preheated to 40°C to 60°C, and then the ceramic coating formation process may be performed.

[0062] After air spraying, the resultant may be cured at a temperature of 230° C. to 280° C. for 10 min to 15 min to form a ceramic coating with a thickness of 10 μm to 80 μm.

[0063] Through the detailed description in combination with the exemplary embodiments above, the ceramic coating of the present invention includes slow-release particles, and therefore, during the cooking process, the release of silicone oil can be slowed down, thereby maintaining a long-lasting non-stick effect.

[0064] Hereinafter, the beneficial effects of the inventive concept will be described in conjunction with specific examples.

[0065] Example 1

[0066] The ceramic coating is formed by the following method.

[0067] S1: 80 wt % of methyltrimethoxysilane and 20 wt % of ethyl orthosilicate are mixed and stirred uniformly to obtain a silane composition of component A;

[0068] S2: 30wt% of Akzo Nobel 1050 (silica sol), 8wt% of titanium dioxide (pigment), 25wt% of kaolin (filler), 3wt% of Tween-80 (emulsifier), 1wt% of water-based modified bentonite (thickener), 0.3wt% of polyoxyethylene ether TRITON X-100 (wetting agent), 20wt% of isopropanol and the balance of deionized water were mixed evenly, then added to a grinder and ground for 2h, fully dispersed and ground to a particle size of not more than 15 microns, to obtain component B slurry;

[0069] S3: 48 parts by weight of formic acid, 48 parts by weight of acetic acid, 1 part by weight of boric acid (buffer), and 0.5 parts by weight of zirconium acetate (catalyst) are uniformly mixed to obtain component C strong acid catalyst;

[0070] S4: Mix 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 with 42 parts by weight of vermiculite with a particle size of 100 to 3000 mesh (sustained-release material), add 3 parts by weight of methoxysilane coupling agent and mix evenly, grind to a particle size of no more than 30 microns, add 0.3 parts by weight of titanate (catalyst), continue grinding to a particle size of no more than 20 microns, and then ultrasonically treat at room temperature of 22°C for 0.5h to obtain a sustained-release particle component D, and the particle size of the sustained-release particle component D obeys a normal distribution.

[0071] S5: The above four components are mixed in order according to the weight ratio of A: B: C: D = 22: 40: 1: 20, and rolled to mature to obtain the ceramic coating. The mixing order and the maturation method are as follows: first, 40 parts by weight of component B and 1 part by weight of component C are mixed evenly, and the pH is adjusted to 4 by component C, and the mixture is rolled and dispersed for 0.5 hours, and then 22 parts by weight of component A are added and shaken evenly, and then 20 parts by weight of component D are added, and the reaction is stirred at a speed of 200 rpm for 8 hours to obtain the desired ceramic coating.

[0072] The non-stick cookware is manufactured by using the ceramic coating as follows.

[0073] S6: Substrate treatment. The stainless steel substrate is sandblasted with 60# brown corundum to form a surface roughness of 3 microns;

[0074] S7: Preheating. Clean the sandblasted substrate and preheat it to 60°C;

[0075] S8: Spraying. The modified ceramic coating is sprayed by air spraying, and the spraying film thickness is 70 microns; the air spraying parameters are as follows: the spraying distance is 160mm; the air pressure is 0.3MPa; and the flow rate is 8L / min.

[0076] S9: Sintering: Curing at 250°C for 10 minutes.

[0077] Through the above method, the non-stick cookware of Example 1 is obtained.

[0078] Example 2

[0079] The difference from Example 1 is that the sustained-release material is bentonite.

[0080] Example 3

[0081] The difference from Example 1 is that the sustained-release material is alpha alumina.

[0082] Example 4

[0083] The difference from Example 1 is that the particle size of the sustained-release particles is less than or equal to 17 microns, and the particle size of the sustained-release particle component D obeys a normal distribution.

[0084] Example 5

[0085] The difference from Example 1 is that the particle size of the sustained-release particles is less than or equal to 12 microns, and the particle size of the sustained-release particle component D obeys a normal distribution.

[0086] Example 6

[0087] The difference from Example 1 is that the particle size of the sustained-release particles is less than or equal to 8 microns, and the particle size of the sustained-release particle component D obeys a normal distribution.

[0088] Example 7

[0089] The difference from Example 1 is that the film thickness is 10 microns.

[0090] Example 8

[0091] The difference from Example 1 is that the film thickness is 40 microns.

[0092] Example 9

[0093] The difference from Example 8 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=30:60:2:5 to prepare the modified ceramic coating.

[0094] Example 10

[0095] The difference from Example 8 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=20:40:1:30 to prepare the modified ceramic coating.

[0096] Embodiment 11

[0097] The difference from Example 1 is that the hydroxy silicone oil is composed of 20 wt % of hydroxy silicone oil with a molecular weight of 800, 60 wt % of hydroxy silicone oil with a molecular weight of 3000 and 20 wt % of hydroxy silicone oil with a molecular weight of 12000.

[0098] Example 12

[0099] The difference from Example 1 is that the silicone oil is composed of 30 wt % of hydroxy silicone oil with a molecular weight of 800, 40 wt % of hydroxy silicone oil with a molecular weight of 3000 and 30 wt % of hydroxy silicone oil with a molecular weight of 12000.

[0100] Embodiment 13

[0101] The difference from Example 1 is that the silicone oil is composed of 25 wt % of hydroxy silicone oil with a molecular weight of 800, 50 wt % of hydroxy silicone oil with a molecular weight of 3000 and 25 wt % of hydroxy silicone oil with a molecular weight of 12000.

[0102] Comparative Example 1

[0103] The difference from Example 1 is that step S4 is omitted. That is, in step S5, components A, B and C are mixed in order according to a weight ratio of A:B:C=22:40:1, and the obtained ceramic material precursor is used to manufacture non-stick cookware.

[0104] Comparative Example 2

[0105] The difference from Example 1 is that 30 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 60 parts by weight of vermiculite.

[0106] Comparative Example 3

[0107] The difference from Example 1 is that 60 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 40 parts by weight of vermiculite.

[0108] The non-stick performance of the non-stick cookware of the above-mentioned Examples 1-13 and Comparative Examples 1-3 was tested, and the test results are shown in the following table.

[0109] plan Long-lasting non-stickiness / times Example 1 21000 Example 2 18000 Example 3 19000 Example 4 20000 Example 5 18000 Example 6 16000 Example 7 11000 Example 8 16000 Example 9 14000 Example 10 25000 Embodiment 11 22000 Example 12 23000 Embodiment 13 25000 Comparative Example 1 500 Comparative Example 2 8000 Comparative Example 3 9000

[0110] Performance index test

[0111] The above-obtained cookware was subjected to a performance test, and the specific performance test method is as follows:

[0112] (1) Long-lasting non-stick test method: refer to 4.2.1 Fried egg non-stick test in GB_T 32095.2-2015. The unit is the number of times. The higher the number, the longer the life. The non-stick result is evaluated once every 1000 times, and the number of times when the non-stickiness reaches Level III is recorded.

[0113] (2) Plane wear resistance test method: GB_T 32095.2-2015 4.3.1 Plane wear resistance test, use 3M7447 scouring pad, apply a force of 15N, the frequency is 33 times / minute, and the scouring pad is replaced every 500 times.

[0114] By comparing and analyzing the embodiments 1-13 of the present invention and the comparative examples 1-3, it is not difficult to find that the conventional ceramic coating in comparative example 1 has a long-lasting non-stickiness of no more than 500 times, the silicone oil in comparative example 2 cannot effectively provide a sustained release effect due to its low content, and the sustained release material content in comparative example 3 is too low, the combined silicone oil is small, and an effective sustained release effect cannot be formed. Compared with comparative examples 1-3, the ceramic coating according to the present invention has excellent long-lasting non-stickiness.

[0115] Although one or more embodiments of the present invention have been described with reference to the drawings, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the claims.

Claims

1. A method for manufacturing a ceramic coating, characterized in that: The method comprises: preparing a ceramic coating precursor and slow-release particles separately and mixing them to prepare a ceramic coating; and forming the ceramic coating on a substrate using a ceramic coating by a layer-forming process, Wherein, the sustained-release particles include a sustained-release material and silicone oil bound to the sustained-release material. Wherein, the sustained-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.

2. The method according to claim 1, characterized in that in, The steps of preparing a ceramic coating precursor include: Prepare material A containing silane substance, material B containing silica sol and filler, material C containing organic acid and slow-release particles; Mixing material B and material C, and adjusting the pH of the mixture to acidic, thereby obtaining a first material; The A material is mixed with the first material, and the mixture is reacted to obtain a ceramic coating precursor.

3. A method for manufacturing a ceramic coating, characterized in that: The method comprises: preparing a ceramic coating; and using the ceramic coating to form the ceramic coating on a substrate by a layer forming process, wherein the step of preparing the ceramic coating comprises: Prepare material A including silane substance, material B including silica sol and filler, material C including organic acid and slow-release particles; Mixing material B and material C, and adjusting the pH of the mixture to acidic, thereby obtaining a first material; The first material is mixed with the A material and the slow-release particles, and the mixture is reacted to obtain a ceramic coating. Wherein, the sustained-release particles include a sustained-release material and silicone oil bound to the sustained-release material. Wherein, the sustained-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.

4. The method according to any one of claims 1 to 3, characterized in that The steps for preparing sustained-release granules include: Provide sustained-release materials and silicone oil; Mixing 35-58 parts by weight of the sustained-release material with 42-60 parts by weight of silicone oil so that the silicone oil is combined with the sustained-release material; and The sustained-release particles combined with silicone oil are ground using a grinding process to obtain sustained-release particles with a particle size less than or equal to 20 microns.

5. The method according to claim 4, characterized in that In the grinding process, silicone oil is mixed evenly with a sustained-release material with a particle size of 100-3000 mesh and ground to a particle size less than or equal to 30 microns. A catalyst is added and the mixture is further ground to a particle size less than or equal to 20 microns to obtain sustained-release particles with a particle size less than or equal to 20 microns.

6. The method according to any one of claims 1 to 3, characterized in that The slow-release particles are contained in 5.15-32.79 parts by weight per 100 parts by weight of the ceramic coating.

7. The method according to claim 4, characterized in that The steps of preparing the sustained-release granules also include: After grinding, the resultant was treated with ultrasonic waves.

8. The method according to any one of claims 1 to 3, characterized in that In terms of weight percentage, the silicone oil includes 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil. Among them, the molecular weight of low molecular weight silicone oil is between 500-1000, the molecular weight of medium molecular weight silicone oil is between 3000-6000, and the molecular weight of high molecular weight silicone oil is between 12000-30000.

9. The method according to any one of claims 1 to 3, characterized in that: The ceramic coating is formed to include at least one layer using a layer forming process, and has a thickness of 10 micrometers to 80 micrometers.

10. The method according to any one of claims 1 to 3, characterized in that The silane substance includes at least one of methyltrimethoxysilane, methyltriethoxysilane and dimethyldimethoxysilane, and the A material also includes tetraethyl orthosilicate. Wherein, in the material A, by weight percentage, the silane substance accounts for 80%-97%, and the tetraethyl orthosilicate accounts for 3%-20%.

Citation Information

Patent Citations

  • Titanium-containing ceramic paint and protective coating

    CN103013193A

  • Water-based inorganic ceramic coating with high weather resistance and high heat absorption as well as preparation and construction methods thereof

    CN115537046A

  • Long-term high-temperature-resistant non-stick ceramic coating as well as preparation method and application thereof

    CN115926498A

  • Modified ceramic coating, composite coating, preparation methods of modified ceramic coating and composite coating, and cooker

    CN116004116A

  • Non-stick ceramic coating and preparation method thereof as well as barbecue tool and preparation method thereof

    CN118638477A