Bio-pollution-resistant water-based colored paint coating for automobiles as well as preparation method and application of bio-pollution-resistant water-based colored paint coating

By using the formula of water-based paint coatings in automotive coatings, combining water-based acrylic resin, polyester modified hydroxyl functional copolymers and environmentally friendly high-to-full sunlight reflectance pigments, the corrosion problem of bio-based pollution on automotive coatings is solved. , realizes efficient thermal energy management and pollution resistance, and maintains the high gloss and leveling of the coating.

CN119060596APending Publication Date: 2024-12-03NIPPON PAINT CHINA +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411454119.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When facing bio-based pollution sources such as bird guano and leaf resins, existing coatings are difficult to effectively resist corrosion, and adjusting the varnish formula to improve pollution resistance will affect the appearance and construction performance of the coating, resulting in VOC emissions. Exceeding the standard or rising costs.

Method used

Use a water-based color paint coating that is resistant to bio-based pollution for automobiles, and its formulation includes aqueous acrylic resin secondary dispersion, aqueous polyester modified hydroxyl functional copolymer emulsion, environmentally friendly water-based high-to-full-solar reflectance pigment color paste, Solvents and additives, by improving the reflective ability of coatings and thermal energy management efficiency, reduce the corrosion ability of bio-based pollutants, and maintain high gloss and leveling.

Benefits of technology

Without affecting the proportion of film-forming resins and VOC emissions of existing coating systems, the coating significantly improves its corrosion resistance to bio-based pollutants, especially the pollution resistance of dark body, and maintains high gloss and Excellent appearance effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005089977230000081
    Figure BDA0005089977230000081
  • Figure BDA0005089977230000091
    Figure BDA0005089977230000091
  • Figure BDA0005089977230000101
    Figure BDA0005089977230000101
Patent Text Reader

Abstract

The invention discloses a bio-pollution-resistant water-based colored paint coating for an automobile as well as a preparation method and application of the bio-pollution-resistant water-based colored paint coating. The water-based colored paint coating is prepared from the following raw materials in parts by weight: 10 to 50 parts of water-based acrylic resin secondary dispersion, 10 to 50 parts of water-based polyester modified hydroxyl functional copolymer emulsion, 5 to 15 parts of amino resin, 1 to 10 parts of environment-friendly water-based high-total-sunlight-reflectance pigment paste, 5 to 30 parts of solvent and auxiliaries, wherein the total mass of the water-based acrylic resin secondary dispersion and the water-based polyester modified hydroxyl functional copolymer emulsion accounts for 50-100 wt% of the total mass of the water-based colored paint coating, and is not 100 wt%. The water-based colored paint coating is beneficial to improving the sunlight reflecting capacity of a coating film on the surface of an automobile body, reducing heat energy conversion, lowering the temperature of the surface of the automobile body and lowering the corrosion capacity of bio-based pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and more specifically to a water-based paint coating for automobiles that is resistant to bio-based pollution, and a preparation method and application thereof. Background Art

[0002] Modern automotive coating systems include electrophoresis, midcoat, color paint, and clearcoat. Each coating plays its own role in the coating system. Electrophoresis protects the body material from corrosion; midcoat covers the electrophoresis color and provides impact resistance; color paint provides color; and clearcoat, as the outermost coating, protects the entire body coating, such as preventing damage to the body coating from natural debris (acid rain, bird droppings, leaf resin), reducing UV damage to the coating, and providing the body with a high gloss and smooth appearance.

[0003] The damage to the car body coating caused by bird droppings and leaf resin dripping in natural falling objects is inevitable in the use of modern cars, and is also one of the important inspection items for car body coatings. The protein in bird droppings that has not been completely digested will destroy the molecular structure of the film-forming substance of the car body coating during the decomposition process under high temperature conditions, thereby causing the coating to be damaged. In addition, the food types of birds in nature are diverse and complex, and the types of protein in their droppings are also different, so the damage to the coating is difficult to completely control. The concentration of chemical substances in leaf resin drippings, such as peach gum and gum arabic, will increase at high temperatures. The concentration of strong acids or strong bases will react chemically with polyurethane, the main film-forming substance of the car body paint coating, causing the coating to lose its effect.

[0004] These two types of natural falling objects are bio-based pollution sources, which we cannot exclude because these natural falling objects are unavoidable when cars are used in the natural environment. Usually, the direction of coating improvement to resist these two types of pollutants is to improve the pollution resistance of the coating by adjusting the formula of the varnish coating, such as improving the density of the film-forming material by adjusting the molecular weight of the film-forming acrylic resin in the varnish formula, or choosing to increase the flexibility of the polyester resin to react with the amino resin, and choosing methyl etherified amino resin to improve the flexibility of the film-forming material. However, these operations will have a great impact on the relevant properties of the varnish coating. For example, the selection of high molecular weight acrylic resin will lead to an increase in the viscosity of the coating. In order to meet the construction viscosity requirements, a large amount of solvents such as butyl acetate need to be used for dilution, which will cause VOC emissions to exceed the standard; the increase in the amount of polyester resin will cause the long-wave value of the appearance data of the varnish coating to decrease; the replacement of methyl etherified amino resin with butyl etherified amino resin will reduce the leveling property of the coating and the weather resistance; in order to solve these problems, we need to add leveling agents and anti-UV and anti-free radical additives to the formula, but these will increase the cost of the formula and affect the construction performance of the coating. Summary of the invention

[0005] In order to at least solve the problem of automobile paint film being polluted by bio-based pollutants, the purpose of the present invention is to provide a water-based paint coating for automobiles that is resistant to bio-based pollution, and a preparation method and application thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A water-based paint coating for automobiles resistant to bio-based pollution, characterized in that the raw materials forming the water-based paint coating contain the following components in parts by weight:

[0008] 10-50 parts of water-based acrylic resin secondary dispersion, 10-50 parts of water-based polyester modified hydroxyl functional copolymer emulsion, 5-15 parts of amino resin, 1-10 parts of environmentally friendly water-based high total solar reflectance pigment paste, 5-30 parts of solvent, and additives;

[0009] The total mass of the aqueous acrylic resin secondary dispersion and the aqueous polyester modified hydroxyl functional copolymer emulsion accounts for 50-100wt% of the total mass of the aqueous paint coating composition, and is not 100wt%.

[0010] Furthermore, the environmentally friendly water-based high total solar reflectance pigment paste is a paste prepared by dispersing the environmentally friendly water-based high total solar reflectance pigment.

[0011] Furthermore, the raw materials contain 1-5% of environmentally friendly water-based high total solar reflectance pigment in terms of mass percentage.

[0012] Furthermore, the environmentally friendly water-based high total solar reflectance pigment has a total solar reflectance of more than 50%.

[0013] Furthermore, the environmentally friendly water-based high total solar reflectance pigment paste is at least one of thermal black paste, thermal orange paste or thermal green paste.

[0014] Furthermore, the environmentally friendly water-based high total solar reflectance pigment paste comprises, by mass percentage:

[0015] 20-25% environmentally friendly water-based high total solar reflectance pigment, 20-25% dispersant, 0.5-1% wetting agent and 50-55% deionized water.

[0016] Furthermore, the environmentally friendly water-based high total solar reflectance pigment is selected from infrared reflective pigments or infrared transmissive pigments.

[0017] Furthermore, the infrared reflective pigment or infrared transmissive pigment is selected from one or more of iron chrome black, bismuth vanadate, cobalt titanium green and chromium oxide green.

[0018] Furthermore, the environmentally friendly water-based high total solar reflectance pigment is selected from one or more of L0086 perylene black pigment, Sicopal PY184 pigment and Ranbar Green I-GN.

[0019] Furthermore, the water-based acrylic resin secondary dispersion has a number average molecular weight of 45,000-85,000, a non-volatile content of 20-50%, and a pH value of 8.0-9.5.

[0020] Further, the aqueous acrylic resin secondary dispersion is selected from at least one of BAYHYDROL A2470, Uacryl2145H, VSC 6276w / 44wA, Setaqua 6803 and Lacper 4702 acrylic emulsions.

[0021] Furthermore, the water-based acrylic resin secondary dispersion is selected from two of BAYHYDROL A2470, Uacryl2145H, Setaqua 6803, and Lacper 4702 acrylic emulsions, wherein the content of one water-based acrylic resin secondary dispersion is 10-20 parts, and the content of the other water-based acrylic resin secondary dispersion is 20-30 parts.

[0022] Furthermore, the aqueous polyester modified hydroxyl functional copolymer emulsion has a number average molecular weight of 60,000-100,000, a polyester content of 5-50 wt%, and a non-volatile content of 35-85 wt%, preferably 42.5-45.5 wt%.

[0023] Furthermore, the aqueous polyester modified hydroxyl functional copolymer emulsion contains 10-20wt% styrene, has a viscosity of 200-2400mPa.s, a pH value of 8.0-9.5, a hydroxyl value of 80-90mgKOH / g, and a density of 1-1.2g / cm 3 .

[0024] Furthermore, the aqueous polyester modified hydroxyl functional copolymer emulsion contains 15wt% styrene, has a viscosity of 200-2400mPa.s, a pH value of 8.0-9.1, a hydroxyl value of 85mgKOH / g, and a density of 1.04g / cm 3 .

[0025] Further, the waterborne polyester modified hydroxyl functional copolymer emulsion is selected from at least one of VIACRYL VSC 6800w / 47wA, YG-SD842 waterborne acrylic modified saturated polyester resin, YG-SP881 waterborne saturated polyester resin, DAOTAN TW6466 / 36WA and DAOTAN TW 6431 / 45WA.

[0026] Further, the aqueous polyester modified hydroxyl functional copolymer emulsion is selected from two of VIACRYL VSC 6800w / 47wA, YG-SD842 aqueous acrylic modified saturated polyester resin, YG-SP881 aqueous saturated polyester resin, DAOTAN TW6466 / 36WA and DAOTAN TW 6431 / 45WA, wherein the content of one aqueous polyester modified hydroxyl functional copolymer emulsion is 10-15 parts, and the content of the other aqueous polyester modified hydroxyl functional copolymer emulsion is 4-10 parts.

[0027] Furthermore, the solvent includes water and an organic solvent.

[0028] Furthermore, the solubility of the organic solvent in water is greater than 20 g / 100 g water, and the boiling point is 150-200°C.

[0029] Furthermore, the organic solvent is selected from alcohol ether solvents and / or alcohol ether ester solvents.

[0030] Furthermore, the solvent contains 5-12 parts of water by weight.

[0031] Furthermore, the auxiliary agent contains 1-5 parts of a dispersant.

[0032] Furthermore, the dispersant is selected from non-ionic dispersants.

[0033] Furthermore, the auxiliary agent also includes at least one of a wetting agent, a leveling agent, a film-forming auxiliary agent, a pH regulator, a defoaming agent, a cosolvent, and a light aging agent.

[0034] Furthermore, the auxiliary agent comprises 0.5-2 parts of a wetting agent, 2-5 parts of a leveling agent, and 2-4 parts of a pH regulator.

[0035] In another aspect, the present invention provides a method for preparing the above-mentioned water-based paint coating for automobiles resistant to bio-based pollution, comprising the following steps:

[0036] The water-based acrylic resin secondary dispersion, the water-based polyester modified hydroxyl functional copolymer emulsion, the solvent and some additives are mixed, and the environmentally friendly water-based high total solar reflectance pigment paste is added. After mixing, the amino resin and the remaining additives are added to obtain the water-based paint coating.

[0037] In another aspect, the present invention provides use of the above-mentioned water-based paint for automobiles resistant to bio-based pollution in the painting of automobile bodies.

[0038] In another aspect, the present invention provides a method for improving the pollution resistance of automobile coatings to bio-based pollutants. In the painting of the automobile body, the above-mentioned automobile water-based paint resistant to bio-based pollution is selected as the paint.

[0039] The beneficial effects of the present invention are as follows:

[0040] In the water-based paint provided in the present invention, the use of water-based high total solar reflectance (TSR) pigment paste helps to improve the reflectivity of the coating film on the surface of the vehicle body to sunlight, reduce heat energy conversion, reduce the temperature of the vehicle body surface, and reduce the corrosion capacity of bio-based pollutants. The water-based paint formula will not affect the film-forming resin ratio of the existing coating system; it will not affect the VOC emissions in the process, and will not affect the visual effect of the appearance of the coating. In particular, it can better improve the bio-based pollution resistance of dark-colored vehicles such as black vehicles; in addition, in the water-based paint, an environmentally friendly water-based high total solar reflectance pigment paste is used to improve the thermal energy management efficiency of the coating system, and the amount of the paste is not significantly different from that of the traditional water-based dispersed paste, and the pigment dispersion method is not significantly different from the dispersing aid used, and there will be no compatibility problems; further, the high gloss and better leveling of the water-based paint coating for automobiles resistant to bio-based pollution are maintained after film coating. DETAILED DESCRIPTION

[0041] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0042] Bio-based pollution sources are natural pollutants of biological origin, including but not limited to leaf resin dripping, bird droppings, etc. In order to improve the pollution of automobile body coatings caused by bio-based pollution sources that cannot be eliminated, and to overcome the problem that it is difficult to ensure the appearance, adhesion, weather resistance and other properties of the coating when adjusting the varnish to improve this problem, the researchers of the present invention have conducted a lot of research.

[0043] The prior art method for improving the bio-based pollution resistance of automobile body coatings is to improve the molecular weight of the film-forming polymer resin in the varnish coating formula and increase the functional group hydroxyl group involved in film formation to improve the compactness of the coating, thereby improving the bio-based pollution resistance of the automobile body coating. However, the following problems may occur when using this method for improvement: increasing the relative molecular weight of the film-forming polyacrylic resin and increasing the amount of functional group hydroxyl group will greatly increase the viscosity of the film-forming resin itself, and the weight proportion of the polymer in the varnish formula is 25-40%, which will cause the viscosity of the final coating to rise sharply. In addition, during the construction and spraying, we need to add a large amount of diluting solvent to reduce the viscosity so as to achieve the viscosity required for on-site construction. The varnish itself is a solvent-based coating, and the solvent used for dilution will eventually evaporate, resulting in an increase in the VOC emission of the final coating, which violates the current environmental protection policy requirements. At the same time, due to the increase in the molecular weight of the polymer acrylic resin, the corresponding amount of curing resin needs to be increased, which will correspondingly reduce the amount of polyester resin in the formula, thereby affecting the gloss and appearance of the final coating.

[0044] The inventor creatively developed a new water-based paint to improve the vehicle body's ability to reflect sunlight, reduce heat conversion, lower the temperature of the vehicle body surface, and reduce the corrosion of bio-based pollutants without adjusting the existing varnish formula and retaining its high gloss and high-grade appearance. The formula of this coating will not affect the film-forming resin ratio of the existing coating system; it will not affect the VOC emissions during the process, and it will not affect the visual appearance of the coating. The coating film has good adhesion, hardness, acid and alkali resistance, water resistance, and pinhole resistance. In particular, it can better improve the bio-based pollution resistance of dark-colored vehicles such as black vehicles.

[0045] Specifically, a specific embodiment of the present invention provides a water-based paint coating for automobiles that is resistant to bio-based pollution. The raw materials for forming the water-based paint coating include the following components in parts by weight:

[0046] 10-50 parts of water-based acrylic resin secondary dispersion, 10-50 parts of water-based polyester modified hydroxyl functional copolymer emulsion, 5-15 parts of amino resin, 1-10 parts of environmentally friendly water-based high total solar reflectance pigment paste, 5-30 parts of solvent, and additives;

[0047] The total mass of the aqueous acrylic resin secondary dispersion and the aqueous polyester modified hydroxyl functional copolymer emulsion accounts for 50-100wt% of the total mass of the aqueous paint coating, and is not 100wt%.

[0048] The water-based color paint is a color paint coating in the automobile coating system. When the water-based color paint is used, no adjustment is required to the clearcoat in the automobile coating system. The water-based color paint will not cause compatibility problems or poor leveling when in contact with the clearcoat, and the high gloss and excellent appearance of the clearcoat can be well maintained.

[0049] In some examples, the total mass of the aqueous acrylic resin secondary dispersion and the aqueous polyester modified hydroxyl functional copolymer emulsion accounts for a percentage of the total mass of the aqueous paint coating, including but not limited to 50-80wt%, 50-70wt%, 50-60wt%, 55-60wt%, etc.

[0050] In some examples, the environmentally friendly water-based high total solar reflectance pigment paste is a paste prepared by dispersing environmentally friendly water-based high total solar reflectance pigment. By using a paint coating containing an environmentally friendly water-based high total solar reflectance pigment paste, the reflectivity of the vehicle body surface to sunlight is improved, heat energy conversion is reduced, the temperature of the vehicle body surface is lowered, and the corrosive ability of bio-based pollutants is reduced.

[0051] In some examples, the environmentally friendly water-based high total solar reflectance pigment has a total solar reflectance of 50% or more.

[0052] In some preferred examples, the environmentally friendly water-based high total solar reflectance pigment paste is at least one of thermal black paste, thermal orange paste or thermal green paste.

[0053] In some examples, the raw material contains 1-5% by mass of an environmentally friendly water-based high total solar reflectance pigment.

[0054] In some specific examples, the environmentally friendly water-based high total solar reflectance pigment paste comprises, by mass percentage:

[0055] 20-25% environmentally friendly water-based high total solar reflectance pigment, 20-25% dispersant, 0.5-1% wetting agent and 50-55% deionized water.

[0056] Exemplarily, the color paste does not contain resin.

[0057] In some examples, the environmentally friendly water-based high total solar reflectance pigment is selected from infrared reflective pigments or infrared transmissive pigments.

[0058] In some more specific examples, the infrared reflective pigment or the infrared transmissive pigment is selected from one or more of iron chrome black, bismuth vanadate, cobalt titanium green and chromium oxide green.

[0059] Exemplarily, the iron chrome black includes but is not limited to CI Pigment Brown 29; the bismuth vanadate includes but is not limited to CI Pigment Yellow 184, Pigment Orange 82, etc.; the cobalt titanium green includes but is not limited to CI Pigment Green 50, etc.; the chromium oxide green includes but is not limited to CI Pigment Green 17, etc.

[0060] In some preferred examples, the pigment is selected from one or more of L0086 perylene black pigment: Paliogen Black L0086 (BASF), Sicopal PY184 pigment (BASF) and Ranbar Green I-GN (Shanghai Jingyan Chemical). Under this condition, the obtained coating has a stronger corrosion resistance to bio-based pollutants and can ensure other excellent properties of the coating film, such as appearance, adhesion, hardness, weather resistance, acid and alkali resistance, etc.

[0061] In some examples, in the formula of the color paste, the dispersant is preferably Dispex Ultra Px4585; and the wetting agent is preferably Surfynol 104A.

[0062] In this embodiment, the addition amount of the exemplary environmentally friendly water-based high total solar reflectance pigment paste includes but is not limited to 5-10 parts, 6-10 parts, 7-10 parts, 8-10 parts, 8 parts, etc. In this case, the above effects are better.

[0063] In some examples, the waterborne acrylic resin secondary dispersion has a number average molecular weight of 45,000-85,000, a non-volatile content of 20-50%, and a pH value of 8.0-9.5.

[0064] In some examples, the water-based acrylic resin secondary dispersion is selected from at least one of BAYHYDROL A2470 (manufactured by Covestro, non-volatile matter 45%), Uacryl 2145H (manufactured by United Cure Chemicals, non-volatile matter 42%), VSC 6276w / 44wA (manufactured by Allnex, non-volatile matter 44%), Setaqua 6803 (manufactured by Allnex, non-volatile matter 24%), and Lacper 4702 acrylic emulsion (manufactured by Wanhua, non-volatile matter 42%).

[0065] Preferably, the water-based acrylic resin secondary dispersion is selected from two of BAYHYDROL A2470 (manufactured by Covestro, non-volatile matter 45%), Uacryl 2145H (manufactured by United Cure Chemicals, non-volatile matter 42%), VSC 6276w / 44wA (manufactured by Allnex, non-volatile matter 44%), Setaqua 6803 (manufactured by Allnex, non-volatile matter 24%), and Lacper 4702 acrylic emulsion (manufactured by Wanhua, non-volatile matter 42%), wherein the content of one water-based acrylic resin secondary dispersion is 10-20 parts, preferably 15-20 parts, and the content of the other water-based acrylic resin secondary dispersion is 20-30 parts, preferably 20-25 parts. At this time, the obtained coating not only has a good effect of resistance to pollution from bio-based pollution sources, but also the use of the water-based acrylic resin secondary dispersion and the water-based polyester modified hydroxyl functional copolymer emulsion can significantly improve the leveling and gloss properties of the coating film.

[0066] In some more preferred examples, the water-based acrylic resin secondary dispersion is selected from a mixture of Lacper 4702 and Setaqua 6803, and the addition amount of Lacper 4702 is 10-20 parts, preferably 15-20 parts, and the addition amount of Setaqua 6803 is 20-30 parts, preferably 20-25 parts. In this case, the comprehensive performance of the coating is better, and the combination of the water-based acrylic resin secondary dispersion and the water-based polyester modified hydroxyl functional copolymer emulsion has a more obvious effect on improving the leveling and gloss of the coating film.

[0067] In some examples, the aqueous polyester modified hydroxyl functional copolymer emulsion has a number average molecular weight of 60,000-100,000, a polyester content of 5-50 wt%, and a non-volatile content of 35-85%, preferably 42.5-45.5 wt%.

[0068] In some examples, the aqueous polyester modified hydroxyl functional copolymer emulsion contains 10-20wt% (preferably 15wt%) styrene, a viscosity of 200-2400mPa.s, a pH value of 8.0-9.5 (preferably 8.0-9.1), a hydroxyl value of 80-90mgKOH / g, and a density of 1-1.2g / cm 3 .

[0069] In some examples, the aqueous polyester modified hydroxyl functional copolymer emulsion is selected from at least one of VIACRYL VSC 6800w / 47wA (manufactured by Allnex, non-volatile matter 47%), YG-SD842 aqueous acrylic modified saturated polyester resin (manufactured by Beijing Sunshine Huide Environmental Protection Technology Co., Ltd., non-volatile matter 47%), YG-SP881 aqueous saturated polyester resin (manufactured by Beijing Sunshine Huide Environmental Protection Technology Co., Ltd., non-volatile matter 81%, propylene glycol methyl ether solution), DAOTAN TW 6466 / 36WA (manufactured by Allnex, non-volatile matter 36%) and DAOTAN TW 6431 / 45WA (manufactured by Allnex, non-volatile matter 44%).

[0070] In some examples, the aqueous polyester modified hydroxyl functional copolymer emulsion is selected from two of VIACRYL VSC 6800w / 47wA, YG-SD842 aqueous acrylic modified saturated polyester resin, YG-SP881 aqueous saturated polyester resin, DAOTAN TW6466 / 36WA and DAOTAN TW 6431 / 45WA, wherein the content of one aqueous polyester modified hydroxyl functional copolymer emulsion is 10-15 parts, and the content of the other aqueous polyester modified hydroxyl functional copolymer emulsion is 4-10 parts. Under this condition, the use of the aqueous acrylic resin secondary dispersion can give the coating film a higher gloss.

[0071] In some preferred examples, the aqueous polyester modified hydroxyl functional copolymer emulsion is a mixture of DAOTAN TW 6466 / 36WA and DAOTAN TW 6431 / 45WA, wherein the addition amount of DAOTAN TW 6466 / 36WA is 10-15 parts, and the addition amount of DAOTAN TW 6431 / 45WA is 4-10 parts, preferably 4-6 parts.

[0072] In some more preferred examples, the waterborne acrylic resin secondary dispersion is a mixture of 10-20 parts of Lacper 4702 and 20-30 parts of Setaqua 6803, and the waterborne polyester modified hydroxyl functional copolymer emulsion is a mixture of 10-15 parts of DAOTANTW 6466 / 36WA and 4-10 parts of DAOTAN TW 6431 / 45WA. The coating film formed at this time has a better appearance (including gloss, leveling, etc.) and pinhole limit, etc.

[0073] In some examples, the total mass of the aqueous acrylic resin secondary dispersion and the aqueous polyester modified hydroxyl functional copolymer emulsion accounts for 50-80wt%, 50-70wt%, 50-60wt%, 55-80wt%, 55-70wt%, 55-60wt%, etc. of the total mass of the aqueous paint coating.

[0074] In this embodiment, the amino resin is used as a cross-linking agent. In some examples, the amino resin includes, but is not limited to, at least one of methyl etherified amino resin, mixed etherified amino resin, and butyl etherified amino resin. In some specific examples, the amino resin is selected from at least one of CYMEL 325 (methyl etherified amino resin manufactured by Allnex), CYMEL 250 (mixed etherified amino resin manufactured by Allnex), and CYMEL 285-100 (butyl etherified amino resin manufactured by Allnex). More preferably, in the raw material, the amount of amino resin added includes, but is not limited to, 5-10 parts, 5-8 parts, 5-6 parts, etc.

[0075] In some examples, the solvent includes water and an organic solvent.

[0076] In some examples, the solubility of the organic solvent in water is greater than 20g / 100g water, and the boiling point is 150-200°C. Exemplary organic solvents are selected from alcohol ether solvents and / or alcohol ether ester solvents. The alcohol ether solvents that can be listed include, but are not limited to, one or more selected from ethylene glycol butyl ether, diethylene glycol butyl ether, ethylene glycol ethyl ether and diethylene glycol ethyl ether; the alcohol ether ester solvents that can be listed include, but are not limited to, selected from ethylene glycol ether acetate, etc. The organic solvent can improve the leveling, gloss, sagging, anti-pinhole and other properties of the coating film, so that the coating has a wider construction window.

[0077] In some examples, the solvent comprises 5-12 parts of water and 5-20 parts of an organic solvent by weight.

[0078] In this embodiment, the auxiliary agent preferably contains 1-5 parts of a dispersant. Preferably, the amount of the dispersant added is 2-4 parts.

[0079] In some examples, the dispersant is selected from non-ionic dispersants. Exemplarily, the dispersant includes, but is not limited to, BYK1190 (BYK Chemical Co., Ltd., Germany), SOLSPERSE2700 (Lubot Specialty Chemicals (Shanghai) Co., Ltd.), etc. The non-ionic dispersant does not produce anions or cations in water, and does not react with anionic resins and cationic resins, which can improve the stability of water-based coatings. In addition, non-ionic dispersants do not produce positive or negative charges in water, have little effect on aqueous emulsions or aqueous secondary dispersions, do not destroy the charge structure of emulsions or secondary dispersions, and also help to improve the stability of water-based coatings.

[0080] It is understood that in this embodiment, other suitable polymer-acceptable additives can be selected according to actual needs. Exemplarily, the additives also include but are not limited to at least one of a wetting agent, a leveling agent, a film-forming aid, a pH adjuster, a defoamer, a cosolvent, and a light aging agent.

[0081] Exemplarily, the wetting agent can be selected from at least one of commercially available TEGO WET 505, DYNOL 607SURFACTANT, etc. The wetting agent is a surfactant with a defoaming function. When used in conjunction with a substrate wetting agent with a strong surface tension reducing effect, a better coating surface tension can be obtained, and a large number of bubbles will not be generated to avoid more adverse surface phenomena during the use of the product. The defoamer-type substrate wetting agent can adopt a defoaming surfactant. Such a defoaming surfactant is known to those skilled in the art. The surface tension reducing substrate wetting agent can adopt a surfactant that reduces surface tension. The surfactant that reduces surface tension is known to those skilled in the art.

[0082] For example, the leveling agent may be selected from commercially available EXXSOL D40 FIUID, SURFYNOL 440, etc., and one type may be selected, or two or more types may be selected for use in combination, as long as the purpose of the invention is not limited.

[0083] For example, the film-forming aid may be selected from at least one of isomeric tridecanol, ethylene glycol ethyl ether acetate, and diethylene glycol ethyl ether acetate.

[0084] Preferably, the amount of the film-forming aid is between 1 and 5 parts, and the optimal amount is 3 to 5 parts.

[0085] Exemplarily, the defoaming agent includes, but is not limited to, BYKETOL-WS and BYKETOL-WA.

[0086] Exemplarily, the light aging agent includes THASORB UV384-2 and the like.

[0087] For example, the pH adjuster preferably has a boiling point below 150° C. As the pH adjuster, an organic amine having a boiling point below 150° C. can be selected, such as organic amines such as dimethylethanolamine and diethanolamine.

[0088] Exemplarily, the cosolvent is a water-dispersible cosolvent. The water-dispersible cosolvent includes alcohol solvents such as n-pentanol, n-hexanol, and glycol ether solvents such as ethylene glycol monohexyl ether. The above cosolvents can be used alone or in combination of two or more.

[0089] In some examples, the total mass parts of the raw materials of the water-based paint coating is 100 parts.

[0090] In some examples, the dry film thickness of the water-based paint after coating is less than 18 μm.

[0091] According to another specific embodiment of the present invention, a method for preparing the above-mentioned water-based paint for automobiles resistant to bio-based pollution is provided, comprising the following steps:

[0092] The water-based acrylic resin secondary dispersion, the water-based polyester modified hydroxyl functional copolymer emulsion, the solvent and some additives are mixed, and the environmentally friendly water-based high total solar reflectance pigment paste is added. After mixing, the amino resin and the remaining additives are added to obtain the water-based paint coating.

[0093] In some specific examples, the preparation method comprises the following steps:

[0094] The water-based acrylic resin secondary dispersion, the water-based polyester modified hydroxyl functional copolymer emulsion, the solvent and the dispersant are mixed, and the environmentally friendly water-based high total solar reflectance pigment paste is added. After mixing, a defoamer, an amino resin, a wetting agent and a pH adjuster are added to obtain the water-based paint coating.

[0095] According to another specific embodiment of the present invention, there is provided the use of the above-mentioned water-based paint for automobiles resistant to bio-based pollution in the painting of automobile bodies.

[0096] Exemplarily, the application includes the following steps:

[0097] Spraying a mid-coat, the water-based color paint and a clear coat (preferably a two-component clear coat) sequentially on the substrate;

[0098] Among them, the spray film thickness of the mid-coat is preferably 15-18μm, and the flash-drying time is 5min; the spray film thickness of the water-based color paint is preferably 12-15μm, the flash-drying time is 5min, the baking temperature is 80℃, and the time is 8min; the spray film thickness of the varnish is preferably 45-50μm, the flash-drying time is 5min, the baking temperature is 140℃, and the time is 30min.

[0099] According to another specific embodiment of the present invention, a method for improving the pollution resistance of automobile coatings to bio-based pollutants is provided. In the painting of the automobile body, the above-mentioned automobile water-based paint resistant to bio-based pollution is selected as the paint.

[0100] The technical solution of the present invention is described below in conjunction with some specific embodiments:

[0101] Example 1

[0102] A water-based paint coating for automobiles that is resistant to bio-based pollution has a raw material formula as shown in Table 1 below.

[0103] The preparation method thereof comprises the following steps:

[0104] Add DAOTAN TW 6466 / 36WA, DAOTAN TW 6431 / 45WA, Lacper 4702, Setaqua6803, diethylene glycol butyl ether, pure water, and SOLSPERSE2700 into a suitable container in sequence and stir for 30 minutes;

[0105] Then slowly add the environmentally friendly water-based high total solar reflectance pigment paste (thermal black paste containing L0086 perylene black pigment) and stir for 30 minutes;

[0106] Slowly adding BYKETOL-WS, CYMEL 325, TEGO Wet 505, DYNOL607SURFACTANT, and DMEA 10 wt % solution in sequence while stirring for 30 minutes to obtain the water-based paint coating for automobiles resistant to bio-based pollution;

[0107] The formula of the above-mentioned environmentally friendly water-based high total solar reflectance pigment paste (thermal black paste containing L0086 perylene black pigment) is, by mass percentage, comprising:

[0108] 22% of environmentally friendly water-based high total solar reflectance pigment Paliogen Black L0086 (L0086 perylene black pigment), 25% of dispersant Dispex Ultra Px4585, 0.8% of wetting agent Surfynol 104A and 52.2% of deionized water.

[0109] Table 1

[0110]

[0111]

[0112] Example 2

[0113] A water-based paint coating for automobiles that is resistant to bio-based pollution, the raw material formula of which is shown in Table 1 above.

[0114] The preparation method thereof comprises the following steps:

[0115] Add DAOTAN TW 6466 / 36WA, DAOTAN TW 6431 / 45WA, Lacper 4702, Setaqua6803, diethylene glycol butyl ether, pure water, and SOLSPERSE2700 into a suitable container in sequence and stir for 30 minutes;

[0116] Then slowly add environmentally friendly water-based high total solar reflectance pigment paste (thermal orange paste containing Sicopal PY184 pigment) and stir for 30 minutes;

[0117] Slowly adding BYKETOL-WS, CYMEL 325, TEGO Wet 505, DYNOL607SURFACTANT, and DMEA 10 wt % solution in sequence while stirring for 30 minutes to obtain the water-based paint coating for automobiles resistant to bio-based pollution;

[0118] The difference between the formula of the above-mentioned environmentally friendly water-based high total solar reflectance pigment color thermal energy orange paste and the paste in Example 1 is that the L0086 perylene black pigment is replaced with Sicopal PY184 pigment, and the other conditions remain unchanged.

[0119] Comparative Example 1

[0120] A water-based paint for automobiles, the raw material formula of which is shown in Table 1 above.

[0121] The preparation method thereof comprises the following steps:

[0122] Add DAOTAN TW 6466 / 36WA, DAOTAN TW 6431 / 45WA, Lacper 4702, Setaqua6803, diethylene glycol butyl ether, pure water, and SOLSPERSE2700 into a suitable container in sequence and stir for 30 minutes;

[0123] Then slowly add carbon black aqueous dispersion paste (containing Raven5000 carbon black paste) and stir for 30 minutes;

[0124] Slowly adding BYKETOL-WS, CYMEL 325, TEGO Wet 505, DYNOL607SURFACTANT and DMEA 10 wt % solution in sequence while stirring for 30 minutes to obtain the water-based paint for automobile;

[0125] The formula of the carbon black aqueous dispersion color paste is different from that of the color paste in Example 1 in that the L0086 perylene black pigment is replaced with Raven 5000 carbon black, and the other conditions remain unchanged.

[0126] Comparative Example 2

[0127] A water-based paint for automobiles, the raw material formula of which is shown in Table 1 above.

[0128] The preparation method thereof comprises the following steps:

[0129] Add DAOTAN TW 6466 / 36WA, DAOTAN TW 6431 / 45WA, Lacper 4702, Setaqua6803, diethylene glycol butyl ether, pure water, and SOLSPERSE2700 into a suitable container in sequence and stir for 30 minutes;

[0130] Then slowly add orange water-based dispersion color paste (containing BASF Pigment Orange L2950) and stir for 30 minutes;

[0131] Slowly adding BYKETOL-WS, CYMEL 325, TEGO Wet 505, DYNOL 607 SURFACTANT and DMEA 10 wt % solution in sequence while stirring for 30 minutes to obtain the water-based paint for automobile;

[0132] The difference between the above orange water-based dispersion color paste and the color paste in Example 1 is that the L0086 perylene black pigment is replaced with BASF Pigment Orange L2950, ​​and the other conditions remain unchanged.

[0133] The color paint coatings of the above-mentioned embodiments and comparative examples are coated, and the coating film is prepared by automatic spraying by a robot, and the spraying equipment is an automatic spraying machine LACTECH.

[0134] The spraying process is as follows: robot spraying → process such as leveling for 5 to 8 minutes → baking at 80℃ for 5 to 8 minutes → baking at 140℃ for 30 minutes.

[0135] Spraying conditions: temperature 24°C, humidity: 65%.

[0136] Among them, the parameters of the above coating preparation equipment are shown in Table 2 below.

[0137] Table 2

[0138] Atomizer Model SAMES707 Hanging cup speed (rpm) 50000 Gun distance (mm) 250 Gun speed (m / s) 0.5 Molding air (mL / min) 600 Interval(mm) 70 Flow rate (mL / min) 260 Voltage(kv) 70

[0139] Among them, the specific coating film preparation coating information parameters are shown in Table 3 below.

[0140] Table 3

[0141] coating Film thickness / μm Flash drying time / min Baking temperature & time IPP G2 white midcoat 15-18 5 / Paint (Example & Comparative Example) 12-15 5 80℃*8min Two-component varnish 45-50 5 140℃*30min

[0142] The results of appearance test (testing standards are ASTM D5767 and ISO 2813) of the coating obtained by the above coating film are shown in Table 4 below.

[0143] Table 4

[0144]

[0145]

[0146] It can be seen from Table 4 above that after the automotive water-based polymer paint coating resistant to bio-based pollution prepared in the embodiment is coated, compared with the comparative example, under the same construction conditions, and the same film thickness, intermediate coating and clear coating conditions, the appearance of the final coating has no obvious difference, and is slightly better than Comparative Example 1; the main resin and the corresponding cured amino resin and the leveling and dispersing aids in the formula of the automotive water-based paint coating resistant to bio-based pollution in the embodiment are not adjusted, only the color paste part in the formula is adjusted, and the color paste formula is a resin-free formula, and there is no adverse compatibility problem with other raw materials of the automotive water-based polymer paint coating resistant to bio-based pollution.

[0147] The water-based polymer paint for automobiles resistant to bio-based pollution prepared in the above embodiment and the product obtained in the comparative example were used to make a film, and their bio-based pollution resistance performance was tested. The test method is:

[0148] Experimental equipment: The equipment used is an artificial irradiation simulation device, and the lamp used is a halogen tungsten lamp (power is 500 watts). By adjusting the radiation light source and the position and angle of the test sample, the temperature of the board prepared in the comparative example reaches 50°C. However, after measurement, the board surface temperature of the embodiment is only 30-40°C under the same radiation light source, board placement angle and time.

[0149] The experimental conditions and reagents are shown in Table 5, which are the experimental standard conditions of Great Wall Motors: GWT D Z14-85:2022-12.

[0150] It should be noted that the experimental conditions were carried out in a hot air oven, which can be used to simulate the evaluation of the ability to resist bio-based pollution in actual scenarios.

[0151] Table 5

[0152] Experimental products Measurement Experimental temperature and humidity Experiment time Pancreatin 0.2ml 50±1℃, relative humidity 30%±5% 0.5h Gum (lignin 1wt% alkaline solution) 0.2ml 50±1℃, relative humidity 30%±5% 0.5h

[0153] The performance rating criteria are shown in Table 6 below.

[0154] Table 6

[0155]

[0156] The test results of the bio-based pollution resistance of the obtained coating are shown in Table 7 below.

[0157] Table 7

[0158] project Example 1 Example 2 Comparative Example 1 Comparative Example 2 Guano resistant Level 1 Level 1 Level 3 Level 3 Resin resistant Level 1 Level 1 Level 3 Level 3 Board temperature & duration 40℃*30min 32℃*30min 50℃*30min 50℃*30min

[0159] Since the embodiment uses an environmentally friendly water-based high total solar reflectance pigment paste, under the same irradiation conditions, the temperature of the plate is 10-15°C lower than that of the coating composition prepared in the comparative example after coating; and under the conditions of the same concentration and composition of guano and resin reagent, the corrosion resistance of the embodiment is higher than that of the comparative example.

[0160] The bio-based pollution-resistant water-based paint for automobiles prepared in the embodiments of the present invention and the products obtained in the comparative examples were used for coating, and the test results of other properties of the obtained coatings are shown in Table 8 below.

[0161] Table 8

[0162]

[0163] It can be seen from Table 8 above that after the automotive water-based bio-based pollution-resistant water-based paint coating prepared in the embodiment is coated, compared with the comparative example, the mechanical properties: adhesion and hardness are no different, and the chemical resistance is qualified. Although the pinhole limit of comparative examples 1-2 is better than that of examples 1 and 2, this difference does not affect the coating performance, because the film thickness of the automotive water-based polymer paint coating composition resistant to bio-based pollution will not exceed 18 μm after coating, so this pinhole limit data will not have any adverse effect on the construction process.

[0164] The water-based paint coating for automobiles resistant to bio-based pollution of the present invention uses an environmentally friendly water-based high total solar reflectance pigment paste to replace a conventional resin-free color paste, thereby retaining the leveling effect, anti-sagging and anti-pinhole performance of the water-based paint coating. Moreover, the compatibility of the water-based paint coating for automobiles resistant to bio-based pollution with a two-component clearcoat will not be affected, so the high gloss and excellent long- and short-wave data of the coating film can be retained without affecting its chemical resistance.

[0165] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A water-based paint coating for automobiles resistant to bio-based pollution, characterized in that: The raw materials for forming the water-based paint coating include the following components by weight: 10-50 parts of water-based acrylic resin secondary dispersion, 10-50 parts of water-based polyester modified hydroxyl functional copolymer emulsion, 5-15 parts of amino resin, 1-10 parts of environmentally friendly water-based high total solar reflectance pigment paste, 5-30 parts of solvent, and additives; The total mass of the aqueous acrylic resin secondary dispersion and the aqueous polyester modified hydroxyl functional copolymer emulsion accounts for 50-100wt% of the total mass of the aqueous paint coating, and is not 100wt%.

2. The water-based paint according to claim 1, characterized in that: The environmentally friendly water-based high total solar reflectance pigment paste is a paste prepared by dispersing environmentally friendly water-based high total solar reflectance pigment; Preferably, the raw material contains 1-5% of environmentally friendly water-based high total solar reflectance pigment by mass percentage; Preferably, the environmentally friendly water-based high total solar reflectance pigment has a total solar reflectance of 50% or more; Preferably, the environmentally friendly water-based high total solar reflectance pigment paste is at least one of thermal black paste, thermal orange paste or thermal green paste; Preferably, the environmentally friendly water-based high total solar reflectance pigment paste comprises, by mass percentage: 20-25% of environmentally friendly water-based high total solar reflectance pigment, 20-25% of dispersant, 0.5-1% of wetting agent and 50-55% of deionized water.

3. The water-based paint according to claim 2, characterized in that: The environmentally friendly water-based high total solar reflectance pigment is selected from infrared reflective pigments or infrared transmissive pigments; More preferably, the infrared reflective pigment or infrared transmissive pigment is selected from one or more of iron chrome black, bismuth vanadate, cobalt titanium green and chromium oxide green; Preferably, the environmentally friendly water-based high total solar reflectance pigment is selected from one or more of L0086 perylene black pigment, Sicopal PY184 pigment and Ranbar Green I-GN.

4. The water-based paint according to claim 1, characterized in that: The water-based acrylic resin secondary dispersion has a number average molecular weight of 45,000-85,000, a non-volatile content of 20-50%, and a pH value of 8.0-9.5; Preferably, the aqueous acrylic resin secondary dispersion is selected from at least one of BAYHYDROL A2470, Uacryl 2145H, VSC6276w / 44wA, Setaqua 6803 and Lacper 4702 acrylic emulsions; Preferably, the aqueous acrylic resin secondary dispersion is selected from two of BAYHYDROL A2470, Uacryl 2145H, Setaqua 6803, and Lacper 4702 acrylic emulsions, wherein the content of one aqueous acrylic resin secondary dispersion is 10-20 parts, and the content of the other aqueous acrylic resin secondary dispersion is 20-30 parts.

5. The water-based paint according to claim 1, characterized in that: The waterborne polyester modified hydroxyl functional copolymer emulsion has a number average molecular weight of 60,000-100,000, a polyester content of 5-50 wt%, and a non-volatile content of 35-85%; Preferably, the aqueous polyester modified hydroxyl functional copolymer emulsion contains 10-20wt% styrene, a viscosity of 200-2400mPa.s, a pH value of 8.0-9.5, a non-volatile content of 42.5-45.5wt%, a hydroxyl value of 80-90mgKOH / g, and a density of 1-1.2g / cm 3 ; Preferably, the aqueous polyester modified hydroxyl functional copolymer emulsion is selected from at least one of VIACRYL VSC 6800w / 47wA, YG-SD842 aqueous acrylic modified saturated polyester resin, YG-SP881 aqueous saturated polyester resin, DAOTAN TW6466 / 36WA and DAOTAN TW 6431 / 45WA; Preferably, the aqueous polyester modified hydroxyl functional copolymer emulsion is selected from two of VIACRYL VSC 6800w / 47wA, YG-SD842 aqueous acrylic modified saturated polyester resin, YG-SP881 aqueous saturated polyester resin, DAOTAN TW 6466 / 36WA and DAOTAN TW 6431 / 45WA, wherein the content of one aqueous polyester modified hydroxyl functional copolymer emulsion is 10-15 parts, and the content of the other aqueous polyester modified hydroxyl functional copolymer emulsion is 4-10 parts.

6. The water-based paint according to claim 1, characterized in that: The solvent comprises water and an organic solvent; Preferably, the solubility of the organic solvent in water is greater than 20 g / 100 g water, and the boiling point is 150-200° C.; Preferably, the organic solvent is selected from alcohol ether solvents and / or alcohol ether ester solvents; Preferably, the solvent contains 5-12 parts of water by weight.

7. The water-based paint according to claim 1, characterized in that: The auxiliary agent comprises 1-5 parts of a dispersant, preferably, the dispersant is selected from a nonionic dispersant; Preferably, the auxiliary agent further comprises at least one of a wetting agent, a leveling agent, a film-forming agent, a pH regulator, a defoaming agent, a cosolvent, and a light aging agent; Preferably, the auxiliary agent comprises 0.5-2 parts of a wetting agent, 2-5 parts of a leveling agent, and 2-4 parts of a pH regulator.

8. The method for preparing a water-based paint coating for automobiles resistant to bio-based pollution according to any one of claims 1 to 7, characterized in that: The steps include: The water-based acrylic resin secondary dispersion, the water-based polyester modified hydroxyl functional copolymer emulsion, the solvent and some additives are mixed, and the environmentally friendly water-based high total solar reflectance pigment paste is added. After mixing, the amino resin and the remaining additives are added to obtain the water-based paint coating.

9. Use of the water-based paint for automobiles resistant to bio-based pollution as claimed in any one of claims 1 to 7 in the painting of automobile bodies.

10. A method for improving the pollution resistance of automobile coatings to bio-based pollutants, characterized in that: In the painting of the automobile body, the automobile water-based color paint resistant to bio-based pollution as claimed in any one of claims 1 to 7 is selected as the color paint.

Citation Information

Patent Citations

  • Dispersed composition, coating composition, coating film, and coloring matter

    CN104937050A

  • Aqueous polymer coating composition for automobiles

    CN110157271A

  • Method for forming multilayer coating film

    CN111655386A

  • Coating system for surface of traffic facility or vehicle and preparation method thereof

    CN115873459A

  • Durable green coating and preparation method thereof

    CN116751486A