Environment-friendly anticorrosive paint and preparation method thereof

By using water-based epoxy resin and two-component paints of barium sulfate, zinc phosphate and other materials, the problems of insufficient adhesion and production complexity of traditional water-based anticorrosion paints under salt spray conditions are solved, and high adhesion and resistance are achieved Corrosiveness and reduces production costs.

CN119060607APending Publication Date: 2024-12-03HEBEI HUAMI RUBBER
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411327295.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional water-based anticorrosion paints have insufficient adhesion under salt spray corrosion conditions, resulting in salt spray infiltration and erosion, affecting service life and aesthetics, and at the same time, they are costly and complex in production processes.

Method used

Use aqueous epoxy resin as the film forming base material, combine barium sulfate, zinc phosphate, and mica powder as filler, and use defoaming agent, flashing agent and wetting agent as auxiliary agent to prepare two-component paint material and stir through dispersion and grinding process improves adhesion and corrosion resistance.

Benefits of technology

The adhesion of the salt spray resistance test within 680 hours was achieved to meet the ASTM standard, reducing production costs and simplifying the process flow, improving the stability and mechanical strength of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of waterborne anticorrosive paint, and provides environment-friendly anticorrosive paint and a preparation method thereof.The environment-friendly anticorrosive paint comprises a component A and a component B. The component A comprises waterborne epoxy resin, a wetting agent, a defoaming agent, a flash rust agent, barium sulfate, zinc phosphate, mica powder and deionized water, and the component B comprises an epoxy curing agent and deionized water. According to the technical scheme, the problems of poor salt mist, high cost and complex preparation process generally existing in water-based paint in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water-based anti-corrosion coatings, and in particular to an environmentally friendly anti-corrosion paint and a preparation method thereof. Background Art

[0002] Anti-corrosion paint is a type of paint used on the surface of an object to protect the inside of the object from corrosion. It is a commonly used type of paint in industrial construction and is widely used in aviation, shipping, chemicals, oil pipelines, steel structures, bridges, oil drilling platforms and other fields. Environmentally friendly anti-corrosion paint is an environmentally friendly and anti-corrosion paint that aims to provide effective protection for various surfaces while reducing the impact on the environment. This type of paint is usually non-toxic, odorless, and environmentally friendly. It is suitable for a variety of application scenarios, such as food workshops, drinking water facilities, chemical equipment, etc., to ensure safe use while protecting the environment.

[0003] Traditional water-based paints generally have the problem of poor salt spray, that is, under salt spray corrosion conditions, water-based paints produce abnormal changes on the surface of the substrate. This problem is mainly due to insufficient adhesion on the surface of the substrate or insufficient adhesion of the primer layer, which causes salt spray to penetrate into the bottom surface of the composite coating and abnormal physical and chemical changes in the contact surface between the primer layer and the substrate. The problem of poor salt spray of water-based paints is a common problem in the coatings industry. Poor salt spray will affect the service life and aesthetics of the coating. Under humid climatic conditions, the erosion of the coating by salt spray will cause the coating to fall off and peel, thereby reducing the corrosion resistance and protective effect of the coating. The problem of poor salt spray will also affect the environmental performance of the coating. The poor salt spray of the coating will not only pollute the environment, but may also affect human health. It is urgent to solve the problem of poor salt spray of water-based coatings.

[0004] In order to solve the above problems, researchers have taken a variety of approaches. On May 25, 2018, Chinese patent CN 108084843 A disclosed a "bottom, middle and surface composite water-based coating for container field and its preparation method", which is made of "graphene + carbon nanotubes + zinc powder + aluminum powder + zinc phosphate" system. However, in the field of coatings, in order to improve performance, only single-layer graphene can be used. The price of single-layer graphene is extremely expensive, and the price per gram is hundreds of yuan. The addition of this material will undoubtedly greatly increase the cost of the paint; at the same time, its composition is relatively complex, divided into primer, intermediate paint and topcoat. Not only is the preparation process complicated, but the use process is also complicated and time-consuming. In addition, Chinese patent CN 107022281 A disclosed on August 8, 2017 an "epoxy anticorrosive primer and its preparation method", which added imported phosphates and imported mica iron oxide, and the prices of these two raw materials are much higher than those of domestic raw materials; and it added iron oxide, talcum powder and inorganic fillers (calcium carbonate and zinc oxide), all of which will gradually settle in the emulsion. In order to solve this problem, it is necessary to add additional anti-settling agents and stabilizers. Summary of the invention

[0005] The invention provides an environmentally friendly anti-corrosion paint, which solves the problems of high cost, emission of harmful substances and insufficient anti-corrosion performance of traditional anti-corrosion paints in the prior art.

[0006] The present invention also proposes the above-mentioned environmentally friendly anti-corrosion paint, which solves the problem of complicated production process and technology of water-based paint in the prior art.

[0007] The technical solution of the present invention is as follows: The present invention provides an environmentally friendly anticorrosive paint, which comprises a component A and a component B; wherein, by weight, the component A comprises the following raw materials: 480-550 parts of waterborne epoxy resin, 2.7-4 parts of wetting agent, 1.9-2.5 parts of defoaming agent, 4.5-6 parts of flash rust agent, 150-185 parts of barium sulfate, 75-85 parts of zinc phosphate, 80-95 parts of mica powder and 145-170 parts of deionized water; The B component includes the following raw materials: 150 parts of epoxy curing agent and 10-25 parts of deionized water; Component A and component B are mixed in a weight ratio of 4.9 to 5.3:1.

[0008] As a limitation, the defoaming agent includes TEGO902W defoaming agent and TEGO810 defoaming agent.

[0009] As another limitation, the environmentally friendly anti-corrosion paint also includes a water-based color paste, and the weight of the water-based color paste is 5 to 10% of the weight of component A.

[0010] As a further limitation, the A component includes the following raw materials: 509.2 parts of waterborne epoxy resin, 3.3 parts of wetting agent, 1.7 parts of TEGO902W defoamer, 0.5 parts of TEGO810 defoamer, 5.4 parts of flash rust agent, 167.9 parts of barium sulfate, 81.3 parts of zinc phosphate, 86.7 parts of mica powder and 160 parts of deionized water; The B component includes the following raw materials: 150 parts of epoxy curing agent and 16.7 parts of deionized water.

[0011] As a third limitation, the water-based epoxy resin is DB4253 water-based epoxy resin, the wetting agent is TEGO270 wetting agent, the flash rust agent is AC18 flash rust agent, and the epoxy curing agent is 4812 epoxy curing agent.

[0012] The present invention also provides a method for preparing the above-mentioned environmentally friendly anticorrosive paint, the preparation method comprising the following steps: (1) Preparation of component A The raw materials in component A are dispersed, stirred and then ground to obtain paint ɑ; (2) Preparation of component B Dispersing the raw materials in component B to obtain liquid material β; (3) Paint matching The paint material ɑ and the liquid material β are mixed and vacuumized to obtain the environmentally friendly anti-corrosion paint.

[0013] As a limitation, in the preparation of the A component, zirconium oxide beads with a diameter of 2 mm are added before grinding, and the weight of the zirconium oxide beads is 15-25% of the weight of the A component.

[0014] As another limitation, in the preparation of the A component, the speed of the dispersion stirring is 600 to 900 r / min, and the time is 8 to 10 min; The grinding procedure is: grinding at 900-1200 r / min for 5-10 min, grinding at 1200-1500 r / min for 5-10 min, and grinding at 1500-1800 r / min for 20-25 min; The fineness of the paint ɑ is 20-25μm.

[0015] As a third limitation, in the preparation of the B component, the dispersion speed is 600 to 900 r / min and the dispersion time is 10 to 15 min.

[0016] As a fourth limitation, in the paint formulation, the mixing speed is 600 to 900 r / min and the mixing time is 5 to 10 min.

[0017] The beneficial effects of the present invention are: ① The environmentally friendly anticorrosive paint provided by the present invention is a water-based two-component paint, which uses epoxy resin as a film-forming base material, precipitated barium sulfate, zinc phosphate, and mica powder as fillers, and defoamers, flash rust agents, and wetting agents as additives. The prepared environmentally friendly anticorrosive paint has a salt spray resistance test time of up to 680 hours, and the adhesion reaches ASTM standard 5B; ② The environmentally friendly anticorrosive paint provided by the present invention is a primer-top paint, which has the advantages of strong adhesion and corrosion resistance of the primer and uniform appearance of the topcoat, good stability, aging resistance, waterproofness, weather resistance and good mechanical strength, so that the product has a wide range of applications; ③ The method for preparing the environmentally friendly anticorrosive paint provided by the present invention adds a defoaming agent according to the test ratio, which ensures that the cost is not increased while reducing the complexity of the production process, thereby improving the production operability, and the production cost is 45.56% of the paint on the market. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Example 1 A method for preparing an environmentally friendly anticorrosive paint This embodiment is a method for preparing an environmentally friendly anti-corrosion paint, and the preparation method comprises the following steps: (1) Weigh 509.2g of DB4253 waterborne epoxy resin, 3.3g of TEGO270 wetting agent, and TEGO902W defoaming agent. 1.7g, AC18 flash rust agent 5.4g, TEGO810 defoamer 0.5g, 3000 mesh precipitated barium sulfate 167.9g, zinc phosphate 81.3g, mica powder 86.7g and deionized water 160g are added into a dispersion container, dispersed and stirred at a speed of 900r / min for 10min, and then added into a sand mill for grinding. Before grinding, 200g of zirconia beads with a diameter of 2mm are added to obtain paint ɑ1 with a fineness of 20-25μm; The grinding procedure is: grinding at 600 r / min for 10 min, grinding at 900 r / min for 10 min, and grinding at 1500 r / min for 25 min; (2) Weigh 150 g of 4812 epoxy curing agent and 16.7 g of deionized water, add them into a dispersion container, and disperse and stir at a speed of 900 r / min for 15 min to obtain liquid material β1.

[0020] (3) Paint preparation: Paint ɑ1 and liquid β1 are mixed at a weight ratio of 5:1, and dispersed at a speed of 600 r / min for 5 min to obtain environmentally friendly anti-corrosion paint θ1.

[0021] The environmentally friendly anti-corrosion paint prepared in this embodiment needs to be vacuum pumped to remove bubbles inside the paint before spraying; and before spraying, the surface of the parts should be completely cleaned, dried, and free of grease and stains. After spraying, the paint needs to be surface-dried for 2 hours before it can be transferred. After five days, the parts are completely dry and the product can be used normally.

[0022] Examples 2 to 5 Preparation methods of environmentally friendly anticorrosive paints Examples 2 to 5 provide a method for preparing an environmentally friendly anticorrosive paint, respectively. The steps are basically the same as those in Example 1, except that the amount of raw materials used and the process parameters are different. See Table 1 for details: Table 1 List of process parameters in Examples 2 to 5

[0023] Example 6 Environmentally friendly anticorrosive paint performance test This example is an environmentally friendly anti-corrosion paint performance test experiment, and the test method is as follows: Salt spray resistance duration: According to the test method specified in GB / T 10125-2021 "Salt Spray Test Standard", spray the test sample on the test plate with a spray thickness of 70 microns, put it into the salt spray test chamber for neutral salt spray test (NSS) to measure the salt spray resistance duration of the paint; Adhesion test: The paint adhesion is tested by the cross-cut method according to the "Determination of paint film adhesion (GB1720-1979)"; Cost accounting: Calculate the price of each kilogram of paint based on the ratio of raw materials required per kilogram of paint weight; Test samples: Test sample 1 is the environmentally friendly anti-corrosion paint θ1 prepared in Example 1 of the present invention. The only difference between test sample 2 and the environmentally friendly anti-corrosion paint θ1 is that 60g of graphite is added to test sample 2. The only difference between test sample 3 and the environmentally friendly anti-corrosion paint θ1 is that the amount of zinc phosphate in test sample 3 is reduced from 81.3g to 60g. Test sample 4 is the paint purchased by the company from outside - 3009 paint.

[0024] The test results are shown in Table 2: Table 2 Performance test results of each test sample

[0025] Results analysis: From the data in Table 2, we can see 1. The environmentally friendly anticorrosive paint θ1 (test sample 1) prepared by the present invention has a salt spray resistance of more than 680 hours, an adhesion grade of 5B, and a raw material price of 40.1 yuan / kg; 2. The salt spray resistance of test sample 2 is about 480h, the adhesion level is 5B, and the raw material price is 56 yuan / kg; 3. The salt spray resistance of test sample 3 is about 240h, the adhesion level is 4B~5B, and the raw material price is 39.8 yuan / kg; 4. The paint purchased by our company from outside - 3009 paint (test sample 4) has a salt spray resistance of about 300 hours, an adhesion level of 3B to 4B, and a raw material price of 88 yuan / kg; In summary, the environmentally friendly anti-corrosion paint prepared by the invention has low cost, and its salt spray resistance test and adhesion can meet the product development requirements.

[0026] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An environmentally friendly anti-corrosion paint, It is characterized in that The environmentally friendly anticorrosive paint comprises component A and component B; wherein, by weight, component A comprises the following raw materials: 480-550 parts of waterborne epoxy resin, 2.7-4 parts of wetting agent, 1.9-2.5 parts of defoaming agent, 4.5-6 parts of flash rust agent, 150-185 parts of barium sulfate, 75-85 parts of zinc phosphate, 80-95 parts of mica powder and 145-170 parts of deionized water; The B component includes the following raw materials: 150 parts of epoxy curing agent and 10-25 parts of deionized water; Component A and component B are mixed in a weight ratio of 4.9 to 5.3:

1.

2. The environmentally friendly anticorrosive paint according to claim 1, It is characterized in that The defoaming agent includes TEGO902W defoaming agent and TEGO810 defoaming agent.

3. The environmentally friendly anticorrosive paint according to claim 1 or 2, It is characterized in that The environmentally friendly anti-corrosion paint also includes a water-based color paste, and the weight of the water-based color paste is 5-10% of the weight of component A.

4. The environmentally friendly anticorrosive paint according to claim 2, It is characterized in that The A component includes the following raw materials: 509.2 parts of waterborne epoxy resin, 3.3 parts of wetting agent, 1.7 parts of TEGO902W defoamer, 0.5 parts of TEGO810 defoamer, 5.4 parts of flash rust agent, 167.9 parts of barium sulfate, 81.3 parts of zinc phosphate, 86.7 parts of mica powder and 160 parts of deionized water; The B component includes the following raw materials: 150 parts of epoxy curing agent and 16.7 parts of deionized water.

5. The environmentally friendly anticorrosive paint according to claim 1, 2 or 4, It is characterized in that The water-based epoxy resin is DB4253 water-based epoxy resin, the wetting agent is TEGO270 wetting agent, the flash rust agent is AC18 flash rust agent, and the epoxy curing agent is 4812 epoxy curing agent.

6. The method for preparing the environmentally friendly anticorrosive paint according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: (1) Preparation of component A The raw materials in component A are dispersed, stirred and then ground to obtain paint ɑ; (2) Preparation of component B Dispersing the raw materials in component B to obtain liquid material β; (3) Paint matching The paint material ɑ and the liquid material β are mixed and vacuumized to obtain the environmentally friendly anti-corrosion paint.

7. The preparation method according to claim 6, It is characterized in that In the preparation of the A component, zirconium oxide beads with a diameter of 2 mm are added before grinding, and the weight of the zirconium oxide beads is 15-25% of the weight of the A component.

8. The preparation method according to claim 6 or 7, It is characterized in that In the preparation of the A component, the speed of the dispersion stirring is 600-900 r / min, and the time is 8-10 min; The grinding procedure is: grinding at 900-1200 r / min for 5-10 min, grinding at 1200-1500 r / min for 5-10 min, and grinding at 1500-1800 r / min for 20-25 min; The fineness of the paint ɑ is 20-25μm.

9. The preparation method according to claim 6 or 7, It is characterized in that In the preparation of the B component, the dispersion speed is 600-900 r / min and the dispersion time is 10-15 min.

10. The preparation method according to claim 6 or 7, It is characterized in that In the paint formulation, the mixing speed is 600-900 r / min and the mixing time is 5-10 min.

Citation Information

Patent Citations

  • Anticorrosion epoxy primer and preparation method thereof

    CN107022281A

  • Bottom-mid-top composite layer waterborne paint applied to field of containers and preparation method of bottom-mid-top composite layer waterborne coating

    CN108084843A

  • Waterborne two-component epoxy primer-topcoat coating and preparation method thereof

    CN114437610A

  • Waterborne two-component epoxy high-gloss primer-topcoat anticorrosive paint and preparation method thereof

    CN116769379A