Single-component modified polysiloxane finish paint as well as preparation method and application thereof

Through the preparation of single-component modified polysiloxane topcoat, the use of hydroxyacrylic resin and bihydroxyl-terminated polysiloxane resin to blend and introduce silane endocrine, the existing polysiloxane topcoat construction problems and The problem of insufficient weather resistance has achieved high-performance anticorrosion coatings for steel structures and concrete.

CN119060633APending Publication Date: 2024-12-03BEIXIN JIABAOLI COATINGS (GUANGDONG) CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411229510.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing polysiloxane topcoats are difficult to adjust paint, have poor heating and early performance during construction, and have poor weather resistance, making it difficult to meet the demand for heavy corrosion protection.

Method used

Moisture-curable modified polysiloxane topcoat is prepared by blending hydroxyacrylic resin with bihydroxyl-terminated polysiloxane resin and introducing silane endocrine to prepare a moisture-curable modified polysiloxane topcoat. , the reaction was carried out using propyltriethoxysilane isocyanate and the organotin catalyst to form a coating with excellent weather resistance.

Benefits of technology

A single-component modified polysiloxane topcoat with convenient construction and excellent performance is realized. It is suitable for heavy corrosion protection of steel structures and concrete, and has significantly improved weather resistance and salt spray resistance, which solves the problem of two-component coatings in construction. puzzles and early performance issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005025660390000071
    Figure BDA0005025660390000071
  • Figure BDA0005025660390000081
    Figure BDA0005025660390000081
Patent Text Reader

Abstract

The invention belongs to the technical field of anticorrosive paint, and discloses single-component modified polysiloxane finish paint as well as a preparation method and application thereof. The single-component modified polysiloxane finish paint comprises silane-terminated modified polysiloxane resin, an auxiliary agent and a solvent, the silane-terminated modified polysiloxane resin is prepared from the following raw materials: hydroxyl-terminated polysiloxane resin, organic silicon modified hydroxyl acrylic resin, isocyanate propyl triethoxy silane and an organic tin catalyst. The silane-terminated modified polysiloxane resin is prepared from the hydroxyl-terminated polysiloxane resin, the organic silicon modified hydroxyl acrylic resin and the isocyanate propyl triethoxy silane, and finally, the modified polysiloxane finish paint with excellent weather resistance is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anti-corrosion coatings, and particularly relates to a single-component modified polysiloxane topcoat and a preparation method and application thereof. Background Art

[0002] At present, the high weather-resistant anti-corrosion topcoats used in heavy-duty anti-corrosion on the market are mainly fluorocarbon topcoats and polysiloxane topcoats. The anti-corrosion durability design period is more than 20 years, and these two topcoats are used. However, due to the harmfulness of fluorine, fluorocarbon topcoats are gradually at risk of being banned. Therefore, the market will gradually pay attention to the development of polysiloxane topcoats.

[0003] At present, the research and development hotspot of polysiloxane topcoat is two-component polysiloxane topcoat. The main paint is composed of polysiloxane oligomers modified by acrylic acid and / or epoxy components, and the curing agent is composed of a cross-linking agent and a catalyst to promote the curing reaction.

[0004] Chinese patent CN113817349A prepares an acrylic modified polysiloxane coating, with an acrylic resin containing active hydrogen functional groups and a polysiloxane intermediate containing phenyl / methyl functional groups as component A, and an organic siloxane containing active hydroxyl groups and reactive glycidoxy groups as component B. Under the action of a catalyst, multiple functional groups have a high crosslinking density, good weather resistance, and good chemical resistance. Because both components contain film-forming resins, the paint adjustment requirements during construction are relatively high, which is not conducive to construction, and the resulting coating has large differences in performance and poor weather resistance.

[0005] Chinese patent CN 113943520A prepares an epoxy resin modified polysiloxane electrostatic conductive coating, which utilizes the curing and cross-linking of epoxy resin and amino polysiloxane resin, uses carbon nanotubes as a conductive agent, has an unobstructed conductive path, and has good chemical resistance, but poor weather resistance.

[0006] Chinese patent CN 116355450A prepares a low-surface-treated polysiloxane coating, which uses silicone intermediates, acrylic monomers, and hydrogenated epoxy resins as component A, and aminosilane oligomers and catalysts as component B. It utilizes the cross-linking reaction between amino groups and double bonds and epoxy groups, as well as the hydrolysis and condensation reaction between siloxane oligomers to cure into a film. It has the characteristics of low surface treatment and the advantage of being recoatable, but has poor weather resistance.

[0007] Chinese patent CN112500791A prepares a one-component moisture-curing polysiloxane coating for color steel tiles, using pure silane-terminated polysiloxane resin as a film-forming substance and hollow glass beads as a reflective insulation filler. It has the advantages of heat resistance, water resistance and weather resistance, but also has poor recoatability, and the hardness after film formation is high and the flexibility is poor.

[0008] Therefore, it is urgent to provide a new anticorrosive topcoat with good weather resistance. Summary of the invention

[0009] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a one-component modified polysiloxane topcoat and a preparation method and application thereof.

[0010] The invention provides a one-component modified polysiloxane topcoat, which is prepared by blending and modifying a hydroxyl-containing acrylic resin and a dihydroxyl-terminated polysiloxane resin, and then introducing silane end-capping. The one-component modified polysiloxane topcoat which can be cured by moisture is suitable for anticorrosive topcoat for concrete and steel structures, and has excellent weather resistance, chemical resistance and salt spray resistance.

[0011] The invention uses hydroxyl-terminated polysiloxane resin, organosilicon-modified hydroxy acrylic resin and isocyanate propyl triethoxysilane to prepare silane-terminated modified polysiloxane resin, and finally forms modified polysiloxane topcoat with excellent weather resistance, and the topcoat forms a film after moisture curing.

[0012] In order to solve the problems of difficult paint mixing, heat generation and poor early performance of two-component polysiloxane coatings during construction, a one-component moisture-curable modified polysiloxane topcoat is prepared, which is convenient to construct and has excellent performance. The one-component modified polysiloxane topcoat of the present invention can be used in heavy-duty anti-corrosion of steel structures and anti-corrosion surfaces of concrete structures, and has excellent weather resistance.

[0013] A first aspect of the present invention provides a one-component modified polysiloxane topcoat.

[0014] Specifically, a one-component modified polysiloxane topcoat includes a silane-terminated modified polysiloxane resin, an additive, and a solvent;

[0015] The raw materials for preparing the silane-terminated modified polysiloxane resin include hydroxyl-terminated polysiloxane resin, organosilicon-modified hydroxyl acrylic resin, isocyanate propyl triethoxysilane and organotin catalyst.

[0016] Preferably, the preparation process of the silane-terminated modified polysiloxane resin comprises the following steps:

[0017] In a protective gas atmosphere, a hydroxyl-terminated polysiloxane resin and an organosilicon-modified hydroxy acrylic resin are mixed and dispersed, and then an organic solvent, isocyanatepropyltriethoxysilane and an organotin catalyst are added to react to obtain the silane-terminated modified polysiloxane resin.

[0018] Preferably, the protective gas atmosphere includes dry nitrogen or dry inert gas (such as argon).

[0019] Preferably, the organic solvent includes at least one of toluene and xylene.

[0020] Preferably, the organotin catalyst is dibutyltin dilaurate.

[0021] Preferably, the reaction temperature is 50-60° C., and the reaction time is 0.5-1 hour.

[0022] Preferably, the hydroxyl-terminated polysiloxane resin is a dihydroxyl-terminated polydimethylsiloxane resin.

[0023] Preferably, the organosilicon-modified hydroxy acrylic resin has hydroxyl groups as functional groups, acrylic acid and polysiloxane as main chains, has good compatibility with hydroxyl-terminated polysiloxane resins, and is not easily delaminated. The organosilicon-modified hydroxy acrylic resin is a commercially available raw material, the main chain structure is mainly CC structure, with a small amount of C-Si structure, and the side chain is hydroxyl.

[0024] Preferably, the one-component modified polysiloxane topcoat comprises, by weight, 30-55 parts of silane-terminated modified polysiloxane resin, 30-58 parts of additives, and 5-20 parts of solvent; further preferably, the one-component modified polysiloxane topcoat comprises, by weight, 40-50 parts of silane-terminated modified polysiloxane resin, 37.31-55.93 parts of additives, and 8-16 parts of solvent.

[0025] Preferably, the auxiliary agent includes at least one of a filler, an anti-settling agent, a wetting and dispersing agent, a leveling agent, a light stabilizer, an ultraviolet light absorber, and a catalyst.

[0026] Preferably, the anti-settling agent is polyamide wax and fumed silica, and the ratio of the two is 1-3:1.

[0027] Preferably, the leveling agent is a fluorosilicone modified acrylic leveling agent.

[0028] Preferably, the solvent is at least one of xylene, propylene glycol methyl ether acetate and cyclohexanone, and further is a mixed solvent of xylene, propylene glycol methyl ether acetate and cyclohexanone.

[0029] Preferably, the filler includes at least one of titanium dioxide and barium sulfate.

[0030] Preferably, the wetting and dispersing agent is AFCONA 5044 from EFCONA Polymers.

[0031] Preferably, the light stabilizer is TINUVIN 1130 from BASF of Germany.

[0032] Preferably, the ultraviolet light absorber is RIASORB UV-1164 produced by Rianlong New Materials Company.

[0033] Preferably, the catalyst is dibutyltin dilaurate, provided by Milliken & Company.

[0034] Preferably, the one-component modified polysiloxane topcoat comprises, by weight, 30-55 parts of silane-terminated modified polysiloxane resin, 35-52 parts of filler, 1-3 parts of anti-settling agent, 0.1-0.3 parts of wetting and dispersing agent, 0.1-0.3 parts of leveling agent, 0.05-0.15 parts of light stabilizer, 0.05-0.15 parts of ultraviolet light absorber, 0.01-0.03 parts of catalyst, and 5-20 parts of solvent; Preferably, the one-component modified polysiloxane topcoat comprises, by weight, 40-50 parts of silane-terminated modified polysiloxane resin, 35-52 parts of filler, 2-3 parts of anti-settling agent, 0.1-0.3 parts of wetting and dispersing agent, 0.1-0.3 parts of leveling agent, 0.05-0.15 parts of light stabilizer, 0.05-0.15 parts of ultraviolet light absorber, 0.01-0.03 parts of catalyst, and 8-16 parts of solvent.

[0035] Preferably, the filler includes 20-30 parts of titanium dioxide and 15-22 parts of barium sulfate.

[0036] The second aspect of the present invention provides a method for preparing a one-component modified polysiloxane topcoat.

[0037] Specifically, a method for preparing a one-component modified polysiloxane topcoat comprises the following steps:

[0038] The components are mixed to obtain the one-component modified polysiloxane topcoat.

[0039] Preferably, the preparation method comprises the following steps:

[0040] Add silane-terminated modified polysiloxane resin, wetting and dispersing agent, leveling agent, solvent, anti-settling agent into a container and disperse them, then add filler and disperse them, finally add light stabilizer, ultraviolet light absorber and catalyst, control the temperature of the production process below 50°C, add solvent to adjust the viscosity, and discharge the material after passing the test.

[0041] The third aspect of the present invention provides an application of a one-component modified polysiloxane topcoat.

[0042] A steel material or concrete, the surface of which is coated with the above-mentioned one-component modified polysiloxane topcoat.

[0043] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0044] (1) The present invention utilizes hydroxyl-terminated polysiloxane resin, silicone-modified hydroxyl acrylic resin, and isocyanatepropyltriethoxysilane to prepare silane-terminated modified polysiloxane resin, and finally forms a modified polysiloxane topcoat with excellent weather resistance, and the topcoat forms a film after moisture curing.

[0045] (2) The one-component modified polysiloxane topcoat of the present invention solves the problems of difficult paint mixing, heat generation and poor early performance in the construction process of two-component polysiloxane coatings. The one-component modified polysiloxane topcoat of the present invention is easy to apply and has excellent performance. The one-component modified polysiloxane topcoat of the present invention can be applied to the heavy-duty anti-corrosion of steel structures and the anti-corrosion surface of concrete structures, and has excellent weather resistance.

[0046] (3) The one-component modified polysiloxane topcoat of the present invention can be moisture-cured and has low requirements on the treatment of the base surface to be coated and the construction environment. DETAILED DESCRIPTION

[0047] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0048] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0049] The sources of raw materials used in the following examples and comparative examples are as follows:

[0050] The silicone-modified hydroxy acrylic resin is provided by Anhui Jiazhi Xinnuo Chemical Co., Ltd., and the product model is JZ9522.

[0051] The wetting and dispersing agent was provided by AFCONA Polymers, and the product model was AFCONA 5044.

[0052] The light stabilizer is provided by BASF of Germany, and the product model is TINUVIN 1130.

[0053] The ultraviolet light absorber is provided by RIASORB New Materials Co., Ltd., and the product model is RIASORB UV-1164.

[0054] The catalyst was provided by Milliken & Company and was dibutyltin dilaurate.

[0055] The leveling agent is a fluorosilicone modified acrylic leveling agent, provided by Anhui Jiazhi Xinnuo Chemical Co., Ltd., and the product model is WE-D8773R.

[0056] The preparation process of the silane-terminated modified polysiloxane resin used in the following examples is as follows:

[0057] In a dry nitrogen environment, the dihydroxy-terminated polydimethylsiloxane resin and the silicone-modified hydroxy acrylic resin were mixed and dispersed for 30 minutes, and then xylene, isocyanatepropyltriethoxysilane and an organic tin catalyst (dibutyltin dilaurate) were added, and the mixture was stirred at 60°C for 1 hour. After the reaction was completed, the stirring was stopped, and the temperature was cooled to room temperature to obtain a silane-terminated modified polysiloxane resin.

[0058] Example 1

[0059] A one-component modified polysiloxane topcoat, composed of the following components in parts by weight: 45 parts of silane-terminated modified polysiloxane resin, 42 parts of filler (24 parts of titanium dioxide, 18 parts of barium sulfate), 1.7 parts of anti-settling agent (composed of polyamide wax and fumed silica in a weight ratio of 2:1), 0.2 parts of wetting dispersant, 0.2 parts of leveling agent, 0.1 parts of light stabilizer, 0.1 parts of ultraviolet light absorber, 0.03 parts of catalyst, and 8 parts of solvent (the solvent is composed of xylene, propylene glycol methyl ether acetate and cyclohexanone in a volume ratio of 1:1:1).

[0060] A method for preparing a one-component modified polysiloxane topcoat comprises the following steps:

[0061] In a dry nitrogen environment, silane-terminated modified polysiloxane resin, wetting and dispersing agent, leveling agent, 80% of solvent, anti-settling agent, are added to a kettle and dispersed for 30 minutes, and then filler is added and dispersed to a fineness of less than 40 μm. Finally, light stabilizer, ultraviolet light absorber and catalyst are added. The temperature of the production process is controlled at 45±2°C, 20% of solvent is added to adjust the viscosity, and the material is discharged to obtain a single-component modified polysiloxane topcoat.

[0062] Example 2

[0063] A one-component modified polysiloxane topcoat, composed of the following components in parts by weight: 40 parts of silane-terminated modified polysiloxane resin, 40 parts of filler (20 parts of titanium dioxide, 20 parts of barium sulfate), 1.7 parts of anti-settling agent (composed of polyamide wax and fumed silica in a weight ratio of 2:1), 0.2 parts of wetting dispersant, 0.2 parts of leveling agent, 0.1 parts of light stabilizer, 0.1 parts of ultraviolet light absorber, 0.03 parts of catalyst, and 8 parts of solvent (the solvent is composed of xylene, propylene glycol methyl ether acetate and cyclohexanone in a volume ratio of 1:1:1).

[0064] A method for preparing a one-component modified polysiloxane topcoat comprises the following steps:

[0065] In a dry nitrogen environment, silane-terminated modified polysiloxane resin, wetting and dispersing agent, leveling agent, 80% of solvent, anti-settling agent, are added to a kettle and dispersed for 30 minutes, and then filler is added and dispersed to a fineness of less than 40 μm. Finally, light stabilizer, ultraviolet light absorber and catalyst are added. The temperature of the production process is controlled at 45±2°C, 20% of solvent is added to adjust the viscosity, and the material is discharged to obtain a single-component modified polysiloxane topcoat.

[0066] Example 3

[0067] A one-component modified polysiloxane topcoat, composed of the following components in parts by weight: 50 parts of silane-terminated modified polysiloxane resin, 45 parts of filler (30 parts of titanium dioxide, 15 parts of barium sulfate), 1.7 parts of anti-settling agent (composed of polyamide wax and fumed silica in a weight ratio of 2:1), 0.2 parts of wetting dispersant, 0.2 parts of leveling agent, 0.1 parts of light stabilizer, 0.1 parts of ultraviolet light absorber, 0.03 parts of catalyst, and 8 parts of solvent (the solvent is composed of xylene, propylene glycol methyl ether acetate and cyclohexanone in a volume ratio of 1:1:1).

[0068] A method for preparing a one-component modified polysiloxane topcoat comprises the following steps:

[0069] In a dry nitrogen environment, silane-terminated modified polysiloxane resin, wetting and dispersing agent, leveling agent, 80% of solvent, anti-settling agent, are added to a kettle and dispersed for 30 minutes, and then filler is added and dispersed to a fineness of less than 40 μm. Finally, light stabilizer, ultraviolet light absorber and catalyst are added. The temperature of the production process is controlled at 45±2°C, 20% of solvent is added to adjust the viscosity, and the material is discharged to obtain a single-component modified polysiloxane topcoat.

[0070] Comparative Example 1

[0071] Compared with Example 1, the difference of Comparative Example 1 is that an equal amount of commercially available silane-modified polyether resin (provided by Wacker, Germany, product model 925) replaces the silane-terminated modified polysiloxane resin in Example 1, and the remaining components and processes are the same as in Example 1.

[0072] Comparative Example 2

[0073] Compared with Example 1, the difference of Comparative Example 2 is that an equal amount of epoxy acrylic modified polysiloxane resin (obtained by a blending reaction of epoxy, acrylic monomers and silicone oligomers) is used to replace the silane-terminated modified polysiloxane resin in Example 1, and the remaining components and processes are the same as those in Example 1.

[0074] Comparative Example 3

[0075] Compared with Example 1, the difference of Comparative Example 3 is that in the preparation process of the silane-terminated modified polysiloxane resin, an equal amount of hydroxyl-containing alkyd resin is used to replace the dihydroxy-terminated polydimethylsiloxane resin, and the other components and processes are the same as those of Example 1.

[0076] Comparative Example 4

[0077] Compared with Example 1, the difference of Comparative Example 4 is that in the preparation process of the silane-terminated modified polysiloxane resin, an equal amount of hydroxyl-containing polyester resin is used to replace the dihydroxy-terminated polydimethylsiloxane resin, and the other components and processes are the same as those of Example 1.

[0078] Comparative Example 5

[0079] Compared with Example 1, the difference of Comparative Example 5 is that in the preparation process of the silane-terminated modified polysiloxane resin, an equal amount of isocyanate (toluene diisocyanate) without a siloxane structure is used to replace isocyanatepropyltriethoxysilane, and the remaining components and processes are the same as those of Example 1. The topcoat prepared in this comparative example does not contain a moisture-curable reactive group, cannot form a film, and has extremely poor weather resistance.

[0080] Product effect testing

[0081] The topcoats prepared in the above Examples 1-3 and Comparative Examples 1-2 were tested in their uncured state and the paint film appearance, weather resistance, alkali resistance, adhesion, and salt spray resistance after curing. The test standards are shown in Table 1, and the test results are shown in Table 2.

[0082] Table 1

[0083] project Test Method Status in container HG / T 4755 Fineness GB / T 1724 Volume solid content GB / T 9272 Paint film appearance HG / T 4755 Weather resistance 3000h GB / T 1865 Storage stability GB / T6753.3 Alkali resistance (saturated calcium hydroxide) JT / T 695 Adhesion GB / T 5210 Salt spray resistance 3000h GB / T 1771

[0084] Table 2

[0085]

[0086]

[0087] As can be seen from Table 1, compared with Example 1, the topcoat adhesion of Comparative Example 1 is significantly worse, and the salt spray resistance for 3000h is also significantly worse. Comparative Example 2 has serious discoloration and severe powdering after 3000h weathering resistance.

[0088] Comparative Examples 3 and 4 were tested for weather resistance according to the above standards. At 1000h, serious discoloration and powdering occurred, which was not the case at 3000h.

[0089] It can be seen that the silane-terminated modified polysiloxane resin of the present invention has the advantages of significantly improving the weather resistance and adhesion effect of the film layer formed by the topcoat.

Claims

1. A one-component modified polysiloxane topcoat, characterized in that: It includes silane-terminated modified polysiloxane resin, additives, and solvents; The raw materials for preparing the silane-terminated modified polysiloxane resin include hydroxyl-terminated polysiloxane resin, organosilicon-modified hydroxyl acrylic resin, isocyanate propyl triethoxysilane and organotin catalyst.

2. The one-component modified polysiloxane topcoat according to claim 1, characterized in that: The preparation process of the silane-terminated modified polysiloxane resin comprises the following steps: In a protective gas atmosphere, a hydroxyl-terminated polysiloxane resin and an organosilicon-modified hydroxy acrylic resin are mixed and dispersed, and then an organic solvent, isocyanatepropyltriethoxysilane and an organotin catalyst are added to react to obtain the silane-terminated modified polysiloxane resin.

3. The one-component modified polysiloxane topcoat according to claim 2, characterized in that: The protective gas atmosphere includes dry nitrogen or dry rare gas.

4. The one-component modified polysiloxane topcoat according to claim 2, characterized in that: The organic solvent comprises at least one of toluene and xylene; and / or the reaction temperature is 50-60° C., and the reaction time is 0.5-1 hour.

5. The one-component modified polysiloxane topcoat according to claim 2, characterized in that: The hydroxyl-terminated polysiloxane resin is a dihydroxyl-terminated polydimethylsiloxane resin.

6. The one-component modified polysiloxane topcoat according to claim 1, characterized in that: By weight, it comprises 30-55 parts of silane-terminated modified polysiloxane resin, 30-58 parts of auxiliary agent and 5-20 parts of solvent.

7. The one-component modified polysiloxane topcoat according to claim 1, characterized in that: The auxiliary agent includes at least one of a filler, an anti-settling agent, a wetting and dispersing agent, a leveling agent, a light stabilizer, an ultraviolet light absorber, and a catalyst.

8. The one-component modified polysiloxane topcoat according to claim 7, characterized in that: The additives include fillers, anti-settling agents, wetting and dispersing agents, leveling agents, light stabilizers, ultraviolet light absorbers and catalysts, and the one-component modified polysiloxane topcoat includes, by weight, 30-55 parts of silane-terminated modified polysiloxane resin, 35-52 parts of fillers, 2-3 parts of anti-settling agents, 0.1-0.3 parts of wetting and dispersing agents, 0.1-0.3 parts of leveling agents, 0.05-0.15 parts of light stabilizers, 0.05-0.15 parts of ultraviolet light absorbers, 0.01-0.03 parts of catalysts and 5-20 parts of solvents.

9. The method for preparing the one-component modified polysiloxane topcoat according to any one of claims 1 to 8, characterized in that: The following steps are involved: The components are mixed to obtain the one-component modified polysiloxane topcoat.

10. A steel material or concrete, characterized in that: The surface of the coating is formed by the one-component modified polysiloxane topcoat described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Single-component moisture-curable polysiloxane coating for color steel tiles

    CN112500791A

  • Acrylic acid modified polysiloxane coating and preparation method thereof

    CN113817349A

  • Carbon nanotube modified polysiloxane coating and preparation method thereof

    CN113943520A

  • Low surface treatment polysiloxane coating and preparation method thereof

    CN116355450A

  • Dual-packaging moisture-curable coating compound

    CN102757719A