High-temperature-resistant reworkable automobile shielding adhesive tape and preparation method thereof

Through the preparation of natural rubber and non-woven fabrics, the problem of insufficient performance and reworkability of acrylate tape at high temperatures is solved, and high-temperature reworkable automobile masking adhesive tape is provided, which improves the performance of the tape and promotes the Environmental friendly.

CN119060642AInactive Publication Date: 2024-12-03CROWN NEW MATERIALS TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411195444.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The acrylate pressure-sensitive tape used in existing automobile manufacturing has poor performance in high temperature environments, is not firmly bonded and has poor reworkability, and the raw materials are derived from non-renewable resources, which affects environmental protection and sustainable development.

Method used

The high-temperature-resistant and reworkable automotive shielding adhesive tape is prepared using natural rubber and non-woven fabrics. Through refining, extrusion, vulcanization, glue coating and drying processes, combined with environmentally friendly solvents and additives, the high-temperature resistance and reworkable properties of the tape are improved. sex.

Benefits of technology

It achieves good bonding performance and reworkability of tape under high temperature environments, avoids degumming, and utilizes renewable resources to facilitate environmental protection and sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060642A_ABST
    Figure CN119060642A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-temperature-resistant reworkable automobile shielding adhesive tape, which comprises the following steps: preparing raw materials, mixing, forming, vulcanizing, cooling, gluing and drying: firstly preparing natural rubber and a non-woven fabric, mixing the natural rubber, extruding and forming to obtain a natural rubber sheet, vulcanizing the natural rubber sheet, and drying to obtain the high-temperature-resistant reworkable automobile shielding adhesive tape. Natural rubber is adopted as a raw material, so that the high temperature resistance of the adhesive tape is improved, the adhesive property is good, the degumming condition is avoided, the natural rubber is a renewable resource, environmental protection and sustainable development are facilitated, and the adhesive tape is suitable for industrial production. And the non-woven fabric is directly coated with glue, so that the adhesive tape is easy to take down after being adhered, and good reworkability is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention belongs to the technical field of adhesive tapes, and in particular relates to a high-temperature resistant reworkable automotive masking adhesive tape and a preparation method thereof. [Background technology]

[0002] Automobile manufacturing is an important part of modern industry, and its production process involves a large number of processes such as component assembly and painting. In these processes, various types of tapes are needed for fixing and masking to ensure the quality and appearance of the product. At the same time, adhesive preparation technology and polymer material science are also indispensable parts of automobile manufacturing, which provide strong support for automobile production. In the existing technology, the tapes used in the automobile manufacturing process are mainly acrylic pressure-sensitive tapes, which have good bonding properties and stability and can meet the use requirements in most cases. However, with the advancement of automobile manufacturing technology, the performance requirements of tapes are getting higher and higher, such as performance and reworkability in high temperature environments. Although the existing acrylic pressure-sensitive tapes meet the needs of automobile manufacturing to a certain extent, there are still some problems and shortcomings in practical applications. First, these tapes have poor performance in high temperature environments and are prone to degumming or weak bonding. Secondly, the reworkability of these tapes is poor. Once they are pasted, it is difficult to remove them, which brings great trouble to the rework operation in the automobile manufacturing process. In addition, the raw materials of these tapes are mainly derived from non-renewable resources such as petroleum, which is not conducive to environmental protection and sustainable development. [Summary of the invention]

[0003] The object of the present invention is to provide a high temperature resistant and reworkable automotive masking adhesive tape which is resistant to high temperatures, has good bonding performance, good reworkability, is beneficial to environmental protection and sustainable development, and a preparation method thereof.

[0004] The present invention is achieved by the following technical solutions:

[0005] A method for preparing a high temperature resistant reworkable automotive masking adhesive tape comprises the following steps:

[0006] S1. Prepare raw materials: including natural rubber and non-woven fabrics;

[0007] S2, mixing: put the natural rubber into an internal mixer, the temperature is 80-90°C, the pressure is 1.5-3MPa, and the mixing time is 30-40 minutes;

[0008] S3, molding: putting the mixed natural rubber into an extruder at a temperature of 120-150°C and a pressure of 2-3MPa to obtain a natural rubber sheet;

[0009] S4, vulcanization: put the obtained natural rubber sheet into a vulcanizer at a temperature of 150-160°C, a pressure of 2.5-3MPa, and a vulcanization time of 20-30 minutes;

[0010] S5, cooling: cooling the vulcanized natural rubber sheet to room temperature;

[0011] S6, glue coating: placing a non-woven fabric on the cooled natural rubber sheet, and coating the non-woven fabric with glue to obtain a natural rubber layer-non-woven fabric layer tape, the glue coating thickness is 0.09-0.1 mm, and the glue coating speed is 5-5.05 m / min;

[0012] S7, drying: putting the natural rubber layer-non-woven fabric layer tape coated with glue in step S6 into an oven at a temperature of 160° C. for 5-10 minutes.

[0013] The method for preparing the high temperature resistant reworkable automotive masking adhesive tape as described above further comprises the following steps:

[0014] S8, cutting: cutting the dried natural rubber layer-non-woven fabric layer tape;

[0015] S9. Packaging: Pack the cut tapes.

[0016] In the method for preparing a high temperature resistant and reworkable automotive masking adhesive tape as described above, the purity of the natural rubber in step S1 is above 95%.

[0017] In the above method for preparing a high temperature resistant reworkable automotive masking adhesive tape, in step S2, the temperature is 80°C, the pressure is 1.5 MPa, and the mixing time is 30 minutes.

[0018] As described above, in the method for preparing a high temperature resistant and reworkable automotive masking adhesive tape, in step S3, the temperature is 120° C. and the pressure is 2 MPa, and a natural rubber sheet with a thickness of 0.5 mm is obtained.

[0019] As described above, in the method for preparing a high temperature resistant and reworkable automotive masking adhesive tape, in step S4, the temperature is 150-160° C., the pressure is 2.5-3 MPa, and the vulcanization time is 20-30 minutes.

[0020] In the method for preparing a high temperature resistant and reworkable automotive masking adhesive tape as described above, in step S6, the coating thickness is 0.09 mm and the coating speed is 5 m / min.

[0021] In the method for preparing a high-temperature resistant and reworkable automotive masking adhesive tape as described above, the prepared raw materials described in step S1 also include environmentally friendly solvents and additives, and the environmentally friendly solvent is a water-based adhesive or a solvent-free adhesive or a biodegradable adhesive or a UV-curable adhesive.

[0022] In the method for preparing the high temperature resistant reworkable automotive masking adhesive tape as described above, the additive is a silane coupling agent.

[0023] A high temperature resistant reworkable automobile masking adhesive tape is prepared by adopting the above-mentioned high temperature resistant reworkable automobile masking adhesive tape preparation method.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] The invention provides a method for preparing a high-temperature resistant and reworkable automobile masking adhesive tape, comprising raw material preparation, mixing, molding, vulcanization, cooling, gluing and drying, firstly preparing natural rubber and non-woven fabric, mixing and extruding the natural rubber to obtain a natural rubber sheet, then vulcanizing the natural rubber sheet, placing a non-woven fabric after cooling and gluing the non-woven fabric to obtain a natural rubber layer-non-woven fabric layer tape, and finally drying. Using natural rubber as the raw material not only improves the high-temperature resistance of the tape, has good bonding performance and avoids degumming, but also natural rubber is a renewable resource, which is beneficial to environmental protection and sustainable development, and directly gluing the non-woven fabric makes the tape easy to remove after being pasted, and has good reworkability.

Brief Description of the Drawings

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below.

[0027] Figure 1 It is a method flow chart of a method for preparing a high temperature resistant reworkable automotive masking adhesive tape in a specific embodiment of the present invention;

[0028] Figure 2 It is a schematic structural diagram of a high temperature resistant and reworkable automotive masking adhesive tape in a specific embodiment of the present invention. [Specific implementation method]

[0029] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] When the embodiments of the present invention mention ordinal numbers such as "first" and "second", unless they do express the meaning of order according to the context, they should be understood as being merely for the purpose of distinction.

[0031] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0032] Specific embodiments, such as Figure 1-2 A method for preparing a high temperature resistant reworkable automotive masking adhesive tape is shown, comprising the following steps:

[0033] Step S1, prepare raw materials: including natural rubber and non-woven fabrics, the selection of non-woven fabrics should ensure good air permeability and moisture absorption; prepare the tape by synthesizing natural rubber, this method can not only improve the high temperature resistance of the tape, so that it can be torn without residual glue after use in a high temperature environment of 200°C, but also solve the problem that the existing acrylic pressure-sensitive tape has poor performance in a high temperature environment, and is prone to degumming or weak bonding. In addition, the tape is prepared by using environmentally friendly raw materials, avoiding the use of non-renewable resources such as petroleum, which is beneficial to environmental protection and sustainable development, and solves the technical problem that the raw materials of the existing tape are mainly derived from non-renewable resources such as petroleum, which is not conducive to environmental protection and sustainable development.

[0034] Step S2, mixing: putting the natural rubber into an internal mixer at a temperature of 80-90° C. and a pressure of 1.5-3 MPa for 30-40 minutes to fully plasticize the natural rubber;

[0035] Step S3, molding: putting the mixed natural rubber into an extruder at a temperature of 120-150° C. and a pressure of 2-3 MPa to obtain a natural rubber sheet;

[0036] Step S4, vulcanization: putting the obtained natural rubber sheet into a vulcanizer at a temperature of 150-160° C., a pressure of 2.5-3 MPa, and a vulcanization time of 20-30 minutes, so that the natural rubber sheet has good elasticity and strength;

[0037] Step S5, cooling: cooling the vulcanized natural rubber sheet to room temperature;

[0038] Step S6, glue coating: Place non-woven fabric on the cooled natural rubber sheet, and apply glue on the non-woven fabric to obtain a natural rubber layer-non-woven fabric layer tape, the glue coating thickness is 0.09-0.1mm, and the glue coating speed is 5-5.05m / min; the tape of the present invention can be directly coated with glue on the non-woven fabric, and can be easily removed when needed, and has excellent reworkability. This is significantly superior to the existing tapes, which have poor reworkability and are difficult to remove once attached.

[0039] Step S7, drying: putting the natural rubber layer 1-non-woven fabric layer 2 tape coated with glue in step S6 into an oven at a temperature of 160° C. for 5-10 minutes, so that the tape has good bonding properties.

[0040] Specifically, the method for preparing the high temperature resistant reworkable automotive masking adhesive tape further comprises the following steps:

[0041] Step S8, cutting: cutting the dried natural rubber layer-non-woven fabric layer tape, preferably, cutting to obtain a tape with a width of 50 mm and a length of 100 mm;

[0042] Step S9, packaging: packaging the cut tape. The packaging material should be selected to ensure that it can protect the tape from contamination and damage. Optionally, the packaging material used is release paper, release film, bubble film or foam plastic.

[0043] Preferably, the purity of the natural rubber in step S1 is above 95%.

[0044] Preferably, in step S2, the temperature is 80°C, the pressure is 1.5 MPa, and the mixing time is 30 minutes, so that the natural rubber is fully plasticized.

[0045] Preferably, in step S3, the temperature is 120°C and the pressure is 2 MPa, and a natural rubber sheet with a thickness of 0.5 mm is obtained.

[0046] Preferably, in step S4, the temperature is 150-160°C, the pressure is 2.5-3MPa, and the vulcanization time is 20-30 minutes, so that the natural rubber sheet has good elasticity and strength.

[0047] Preferably, in step S6, the glue coating thickness is 0.09 mm and the glue coating speed is 5 m / min.

[0048] Specifically, the prepared raw materials described in step S1 also include environmentally friendly solvents and additives, and the environmentally friendly solvents are water-based adhesives, solvent-free adhesives, biodegradable adhesives, or UV-curable adhesives. The selection of environmentally friendly solvents should ensure that they are non-toxic and harmless, and the selection of additives should ensure that they can improve the high temperature resistance and reworkability of the tape. Water-based adhesives are adhesives that use water as a dispersion medium, do not contain organic solvents, are environmentally friendly, and are safe to use. Solvent-free adhesives (also known as reactive adhesives): do not contain solvents, do not cause pollution and harm, and are suitable for a variety of industrial uses. UV-curable adhesives: cured by ultraviolet irradiation, do not contain volatile organic compounds (VOCs), have a fast curing speed, and are suitable for automated production lines. Biodegradable adhesives: use degradable polymers as base resins, which can decompose in a natural environment and reduce environmental pollution.

[0049] More specifically, the additive is a silane coupling agent. As an auxiliary agent, the high temperature resistance and bonding strength of the adhesive can be improved.

[0050] The high temperature resistant reworkable automobile masking adhesive tape of the present invention is prepared by adopting the high temperature resistant reworkable automobile masking adhesive tape preparation method as described above.

[0051] The above is an implementation method provided in combination with specific content, and it is not considered that the specific implementation of the present invention is limited to these descriptions. At the same time, due to different industry naming, it is not limited to the above naming, nor is it limited to English naming. Any similarity or similarity with the method, structure, etc. of the present invention, or a number of technical deductions or substitutions made under the premise of the concept of the present invention, shall be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a high temperature resistant reworkable automotive masking adhesive tape, characterized in that: The following steps are involved: S1. Prepare raw materials: including natural rubber and non-woven fabrics; S2, mixing: put the natural rubber into an internal mixer, the temperature is 80-90°C, the pressure is 1.5-3MPa, and the mixing time is 30-40 minutes; S3, molding: putting the mixed natural rubber into an extruder at a temperature of 120-150°C and a pressure of 2-3MPa to obtain a natural rubber sheet; S4, vulcanization: put the obtained natural rubber sheet into a vulcanizer at a temperature of 150-160°C, a pressure of 2.5-3MPa, and a vulcanization time of 20-30 minutes; S5, cooling: cooling the vulcanized natural rubber sheet to room temperature; S6, glue coating: placing a non-woven fabric on the cooled natural rubber sheet, and coating the non-woven fabric with glue to obtain a natural rubber layer-non-woven fabric layer tape, the glue coating thickness is 0.09-0.1 mm, and the glue coating speed is 5-5.05 m / min; S7, drying: putting the natural rubber layer-non-woven fabric layer tape coated with glue in step S6 into an oven at a temperature of 160° C. for 5-10 minutes.

2. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 1, characterized in that: The following steps are also included: S8, cutting: cutting the dried natural rubber layer-non-woven fabric layer tape; S9. Packaging: Pack the cut tapes.

3. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 1, characterized in that: The purity of the natural rubber in step S1 is above 95%.

4. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 1, characterized in that: In step S2, the temperature is 80°C, the pressure is 1.5 MPa, and the mixing time is 30 minutes.

5. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 1, characterized in that: In step S3, the temperature is 120°C and the pressure is 2 MPa, and a natural rubber sheet with a thickness of 0.5 mm is obtained.

6. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 1, characterized in that: In step S4, the temperature is 150-160°C, the pressure is 2.5-3MPa, and the vulcanization time is 20-30 minutes.

7. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 1, characterized in that: In step S6, the glue coating thickness is 0.09 mm and the glue coating speed is 5 m / min.

8. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 1, characterized in that: The prepared raw materials described in step S1 also include environmentally friendly solvents and additives, and the environmentally friendly solvent is a water-based adhesive, a solvent-free adhesive, a biodegradable adhesive, or a UV-curable adhesive.

9. The method for preparing a high temperature resistant reworkable automotive masking adhesive tape according to claim 8, characterized in that: The additive is a silane coupling agent.

10. A high temperature resistant reworkable automotive masking adhesive tape, characterized in that: The adhesive tape is prepared by the method for preparing the high temperature resistant and reworkable automotive masking adhesive tape as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Pressure sensitive adhesive tape for high-temperature resistant masking and preparation method thereof

    CN103571369A

  • High-performance masking tape and preparation method thereof

    CN108893076A

  • Masking tape and masker using it

    JP2004024958A