Leather with conductive gradient structure as well as preparation method and application of leather
By introducing conductive materials such as hydrotalcite, carbon black and polypyrrole into the leather, the conductive gradient structure is constructed, which solves the problem that the conductive materials only have surfaces, improves the electromagnetic shielding performance and durability, and is suitable for intelligent wearable materials.
Patent Information
- Application Number
- CN202411175671.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-26
AI Technical Summary
In the prior art, when preparing electromagnetic shielded leather, conductive materials only exist on the surface of the material, which easily destroys the softness and durability of the leather, and the preparation conditions are strict, limiting its application in intelligent wearable materials.
By adding conductive materials such as hydrotalcite, carbon black and polypyrrole to the pretreated leather, it uses ultrasound or physical machinery to make it enter the interior of the leather collagen fibers, and build a conductive gradient structure to form a continuous conductive network to enhance the mediation of electromagnetic waves. Electrical loss.
It has achieved improvement in electromagnetic shielding performance, reduced the resistance of leather, enhanced its absorption loss on electromagnetic waves, avoided reflection loss, and was simple to operate and low production cost, which is suitable for large-scale production.
Smart Images

Figure CN119061212A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of leather tanning, and relates to leather with a conductive gradient structure and a preparation method and application thereof. Background Art
[0002] Leather has abundant multi-scale pores, which can provide a suitable propagation channel for incident electromagnetic waves; the complex three-dimensional network cross-linked structure in the fiber can form multiple diffuse reflections of electromagnetic waves. The synergistic effect of the two can effectively reduce the number of emitted electromagnetic waves and achieve the purpose of electromagnetic shielding. In addition, leather collagen fibers are rich in carboxyl and amino groups. They have opposite charges and can act as electric dipoles to enhance the dielectric loss of collagen fibers to incident electromagnetic waves. At the same time, carboxyl and amino groups can be used as active groups to chemically bond with conductive materials, which is convenient for building a stable and continuous conductive network, increasing the number of electromagnetic waves entering the leather, which is beneficial to the leather's absorption of electromagnetic waves.
[0003] The prior art for the preparation of electromagnetic shielding leather usually involves coating or filtering a conductive material on the leather surface to prepare a conductive coating, thereby obtaining electromagnetic shielding leather. For example, a dispersion of nano-metal powders (silver, copper, silver-coated copper, ferroferric oxide, nickel and zinc) and a film-forming agent are sprayed on the leather surface, and a leather material with electromagnetic shielding performance is obtained after drying (CN105219895A); multi-walled carbon nanotube-coated metal nanoparticles are filtered and dip-coated on a leather substrate to develop a lightweight, high-performance electromagnetic shielding leather with an excellent electromagnetic shielding performance of 76dB. However, the above method has harsh preparation conditions and cumbersome procedures, and the conductive material only exists on the surface of the material, which easily destroys the softness and durability of the leather itself, limiting its application in intelligent wearable materials. Therefore, it is of great significance to provide an electromagnetic shielding leather that can give full play to the advantages of leather materials in the field of electromagnetic shielding, directly construct a conductive network inside the leather, and has excellent performance. Summary of the invention
[0004] The object of the present invention is to provide a leather with a conductive gradient structure and a preparation method and application thereof. The leather uses conductive materials such as hydrotalcite, carbon black, polypyrrole, etc. to enter the interior of the leather collagen fibers through ultrasonic or physical mechanical action to modify the leather collagen fibers. This method can increase the porosity of the leather fiber structure, which is convenient for electromagnetic waves to be reflected multiple times inside the leather; at the same time, the conductive material constructs a conductive network inside the collagen fibers, so that the resistance of the prepared electromagnetic shielding leather is reduced, which is conducive to enhancing the dielectric loss of electromagnetic waves. This method can give the finished leather thermal stability and electromagnetic shielding performance.
[0005] In a first aspect, the present invention provides a method for preparing leather having a conductive gradient structure, comprising: a method for preparing leather having a conductive gradient structure, characterized in that it comprises: adding a dielectric material having a microwave absorbing property to a pretreated acid leather bath liquid for a first immersion treatment to obtain dielectric leather;
[0006] placing the dielectric leather in a solution containing a conductive material for a second immersion treatment to obtain conductive leather;
[0007] The conductive leather is placed in a solution containing polymer monomers for a third immersion treatment, and an oxidant is added to carry out polymerization reaction to obtain leather with a conductive gradient structure.
[0008] Furthermore, in the method for preparing leather with a conductive gradient structure of the present invention, the pretreatment is pickling treatment;
[0009] The pH of the bath in the pickling treatment is 2.5 to 3.5.
[0010] Furthermore, in the method for preparing leather with a conductive gradient structure of the present invention, the dielectric material with wave absorbing properties is hydrotalcite;
[0011] The mass of the hydrotalcite is 5% to 10% of the mass of water.
[0012] Furthermore, in the method for preparing leather with a conductive gradient structure of the present invention, the first dipping treatment comprises: rotating, adjusting pH, and standing;
[0013] The pH is adjusted to 4-6;
[0014] The rotation time is 2 to 4 hours;
[0015] The standing time is 6 to 24 hours.
[0016] Furthermore, in the method for preparing leather with a conductive gradient structure described in the present invention, the conductive material is carbon black.
[0017] Furthermore, in the method for preparing leather with a conductive gradient structure of the present invention, the second dipping treatment comprises: adjusting pH, ultrasound, and rotation;
[0018] The pH value is adjusted to 5.5 to 7;
[0019] The ultrasound time is 15 min;
[0020] The rotation time is 2 to 6 hours.
[0021] Furthermore, in the method for preparing leather with a conductive gradient structure described in the present invention, the polymer monomer is pyrrole, and the oxidant is ferric chloride.
[0022] Furthermore, in the method for preparing leather with a conductive gradient structure of the present invention, the third dipping treatment comprises: rotating;
[0023] The rotation time is 1 to 2 hours.
[0024] In a second aspect, the present invention also provides leather with a conductive gradient structure prepared by the method for preparing leather with a conductive gradient structure.
[0025] Furthermore, the SEM image of the cross-section of the leather with a conductive gradient structure provided by the present invention includes hydrotalcite with a hexagonal lamellar structure, carbon black with a spherical structure, and polypyrrole wrapped around the fibers, which indicates that the conductive material has entered the interior of the leather and is stably present on the collagen fibers.
[0026] In a third aspect, the present invention provides use of leather having a conductive gradient structure for preparing electromagnetic shielding materials.
[0027] Furthermore, the electromagnetic shielding effectiveness of the leather with a conductive gradient structure provided by the present invention is 45dB, and the electromagnetic shielding performance of the leather with a conductive gradient structure is mainly based on absorption loss, which effectively avoids the reflection loss of highly conductive materials and is more conducive to reducing electromagnetic pollution.
[0028] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects or advantages:
[0029] The present invention allows hydrotalcite to penetrate into the leather interior by impregnation, and the hydroxyl group on the hydrotalcite and the metal ion are combined with the amino group and the carboxyl group on the leather collagen to carry out chemical bond, thereby improving the dielectric property of the leather, and the collagen fiber structure of the leather is appropriately relaxed, thereby creating favorable conditions for the deep penetration of carbon black and pyrrole monomers. In addition, the hydrotalcite dielectric leather obtained has more active sites than the fiber of the acid leather, and can be electrostatically adsorbed and chemically bonded with modified carbon black, so as to be convenient to build a continuous conductive network inside. Finally, pyrrole is infiltrated into the interior and in-situ polymerized on the fiber, so that the defects of the nano conductive material can be filled, and polypyrrole is evenly covered on the collagen fiber, effectively enhancing the conductivity.
[0030] The polypyrrole / carbon black / hydrotalcite conductive leather prepared by the present invention constructs a conductive gradient structure of high conductivity (conductive polymer layer)-good conductivity (conductive nanomaterial layer)-dielectric (wave absorbing material layer) inside the leather fiber, which can effectively reduce the surface resistance of the leather, form a good impedance match with the air, and allow electromagnetic waves to fully enter the leather for loss. The gradient structure can enable the leather to obtain good electromagnetic shielding performance while reducing reflection loss and increasing absorption loss, thereby solving the problem that the reflection loss of high-conductivity electromagnetic shielding materials is higher than the absorption loss.
[0031] The polypyrrole / carbon black / hydrotalcite conductive leather prepared by the present invention has a continuous and stable three-dimensional conductive network inside, which can increase the transmission path of electromagnetic waves inside the leather, so that electromagnetic energy is further dissipated in the form of heat energy, and effectively avoid the transmission of electromagnetic waves. The method is simple to operate, does not require expensive equipment, has low production cost, and can be used for large-scale production. Therefore, the present invention provides a simple method for preparing intelligent leather, which is of great significance to the reform and development of the traditional leather industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The cross-sectional optical photos and SEM images of polypyrrole / carbon black / hydrotalcite conductive leather, carbon black / hydrotalcite conductive leather, hydrotalcite dielectric leather and acid leather with conductive gradient structure. Among them, A is the cross-sectional image of acid leather; B is the cross-sectional SEM image of acid leather at 5μm scale; C is the cross-sectional SEM image of acid leather at 100nm scale; D is the cross-sectional image of hydrotalcite dielectric leather; E is the cross-sectional SEM image of hydrotalcite dielectric leather at 2μm scale; F is the cross-sectional SEM image of hydrotalcite dielectric leather at 500nm scale; G is the cross-sectional image of carbon black / hydrotalcite conductive leather; H is the cross-sectional SEM image of carbon black / hydrotalcite conductive leather at 5μm scale; I is the cross-sectional SEM image of carbon black / hydrotalcite conductive leather at 1μm scale. Cross-sectional SEM image of polypyrrole / carbon black / hydrotalcite conductive leather; J is cross-sectional SEM image of polypyrrole / carbon black / hydrotalcite conductive leather; K is cross-sectional SEM image of polypyrrole / carbon black / hydrotalcite conductive leather at 2μm scale; L is cross-sectional SEM image of polypyrrole / carbon black / hydrotalcite conductive leather at 200nm scale; SP is acid leather; LDHs-L is hydrotalcite dielectric leather; CB / LDHs-L is carbon black / hydrotalcite conductive leather; PPy / CB / LDHs-L is polypyrrole / carbon black / hydrotalcite conductive leather.
[0033] Figure 2 The shrinkage temperature diagram of polypyrrole / carbon black / hydrotalcite conductive leather, carbon black / hydrotalcite conductive leather, hydrotalcite dielectric leather and acid leather with conductive gradient structure.
[0034] Figure 3 This is a graph of the electromagnetic shielding efficiency of polypyrrole / carbon black / hydrotalcite conductive leather, carbon black / hydrotalcite conductive leather, hydrotalcite dielectric leather and acid leather with a conductive gradient structure.
[0035] Figure 4 Shielding coefficient diagram of polypyrrole / carbon black / hydrotalcite conductive leather, carbon black / hydrotalcite conductive leather and hydrotalcite dielectric leather with conductive gradient structure. DETAILED DESCRIPTION
[0036] The technical scheme of the present invention is described below in conjunction with the embodiments, but the present invention is not limited to the following embodiments. The experimental methods and detection methods described in each embodiment are conventional methods unless otherwise specified; the reagents and materials described are all commercially available unless otherwise specified.
[0037] Example 1
[0038] This embodiment provides a method for preparing electromagnetic shielding leather with a conductive gradient structure.
[0039] 1. Preparation of hydrotalcite dielectric leather
[0040] 30g goat skin (bare skin) is put into a rotary drum, and then 60mL of water and 4.2g of salt are added successively as body lotion. The pH value of the body lotion in the rotary drum is regulated repeatedly using a 1mol / L formic acid solution in small quantities until the pH value of the body lotion is 3. The rotary drum is rotated for 30min, and the pickling of the goat skin is completed to obtain acid skin. Then 4.8g of hydrotalcite is added into the rotary drum, and after rotating for 4h, the sodium bicarbonate solution of 1mol / L is added to adjust the pH value to 6, and the hydrotalcite is left to stand for 24h so that the collagen fibers of the goat skin are evenly combined to obtain hydrotalcite dielectric leather.
[0041] 2. Preparation of carbon black / hydrotalcite conductive leather
[0042] The hydrotalcite dielectric leather was placed in a 1 mol / L conductive carbon black aqueous solution, and the pH of the conductive carbon black aqueous solution was adjusted to 7 using a 1 mol / L sodium bicarbonate solution. After ultrasonic treatment for 15 minutes, the drum was rotated for 4 hours to combine the conductive carbon black with the collagen fibers through physical and mechanical action to obtain the carbon black / hydrotalcite conductive leather.
[0043] 3. Preparation of polypyrrole / carbon black / hydrotalcite conductive leather
[0044] In an environment of 5°C, 1 mol / L pyrrole monomer was dispersed in a mixed solution of 20 mL ethanol and 20 mL water to obtain a mixed solution. Carbon black / hydrotalcite conductive leather was placed in the mixed solution, the drum was rotated vigorously for 2 hours, 1 mol / L ferric chloride solution was added, and the drum was slowly rotated for 6 hours to obtain polypyrrole / carbon black / hydrotalcite conductive leather.
[0045] Figure 1The cross-sectional optical photographs and SEM images of the polypyrrole / carbon black / hydrotalcite conductive leather (PPy / CB / LDHs-L), carbon black / hydrotalcite conductive leather (CB / LDHs-L), hydrotalcite dielectric leather (LDHs-L) and acid leather (SP) with conductive gradient structure prepared in this embodiment. It can be seen intuitively from the cross-sectional optical photographs that the acid leather cross section is yellow-white ( Figure 1 A in the figure), the cross section of the hydrotalcite dielectric leather is uniform orange-yellow ( Figure 1 D), the cross section of carbon black / hydrotalcite conductive leather is black ( Figure 1 G in the figure), the black color of the cross section of the polypyrrole / carbon black / hydrotalcite conductive leather is further deepened ( Figure 1 The above phenomenon shows that the conductive materials such as hydrotalcite, carbon black and polypyrrole evenly enter the leather collagen fibers and modify the leather collagen fibers. The SEM images of the cross section at different scales further confirm this conclusion. The collagen fibers in the SEM image of the acid leather cross section are closely arranged ( Figure 1 B and C in the figure); In the SEM image of the cross section of the hydrotalcite dielectric leather, it can be found that there are hexagonal lamellar structures of hydrotalcite on the leather collagen fibers ( Figure 1 E and F in the figure); In the SEM image of the cross section of the carbon black / hydrotalcite conductive leather, there are both hexagonal lamellar hydrotalcite and spherical carbon black ( Figure 1 H and I in the figure); the SEM image of the cross section of the polypyrrole / carbon black / hydrotalcite conductive leather includes hexagonal lamellar structure of hydrotalcite, spherical structure of carbon black and polypyrrole ( Figure 1 K and L in the figure, which all indicate that the conductive material enters the leather and exists stably on the collagen fibers.
[0046] Figure 2 The shrinkage temperature diagram of the polypyrrole / carbon black / hydrotalcite conductive leather, carbon black / hydrotalcite conductive leather, hydrotalcite dielectric leather and acid leather with conductive gradient structure prepared in this embodiment. It can be seen from the figure that the hydrotalcite dielectric leather has the highest shrinkage temperature, which can reach 85°C; with multiple loadings of conductive materials, the shrinkage temperature of the leather decreases, but the final shrinkage temperature of the polypyrrole / carbon black / hydrotalcite conductive leather can also reach 77°C, which is much higher than the shrinkage temperature of the acid leather, indicating that the conductive leather prepared by this preparation method has good moisture and heat resistance stability.
[0047] Figure 3The electromagnetic shielding efficiency diagram of polypyrrole / carbon black / hydrotalcite conductive leather, carbon black / hydrotalcite conductive leather, hydrotalcite dielectric leather and acid leather with conductive gradient structure prepared in this embodiment. It can be seen from the figure that the combination of collagen fiber with hydrotalcite, carbon black and polypyrrole can effectively improve the electromagnetic shielding performance of leather, and with the complete construction of conductive gradient, the electromagnetic shielding efficiency of polypyrrole / carbon black / hydrotalcite conductive leather is significantly improved, up to 45dB.
[0048] Figure 4 The shielding coefficient diagram of the polypyrrole / carbon black / hydrotalcite conductive leather, carbon black / hydrotalcite conductive leather, and hydrotalcite dielectric leather with a conductive gradient structure prepared in this embodiment. It can be seen from the figure that the conductive gradient structure of high conductivity (conductive polymer layer, polypyrrole layer)-good conductivity (conductive nanomaterial layer, carbon black layer)-dielectric (wave absorbing material layer, hydrotalcite layer) makes the absorption coefficient in the electromagnetic shielding process greater than the reflection coefficient, indicating that the electromagnetic shielding performance of the polypyrrole / carbon black / hydrotalcite leather is mainly based on absorption loss, effectively avoiding the reflection loss of the high conductive material, and is more conducive to reducing electromagnetic pollution.
[0049] Table 1 Comparison of surface resistance of acid leather, hydrotalcite dielectric leather, carbon black / hydrotalcite conductive leather and polypyrrole / carbon black / hydrotalcite conductive leather
[0050]
[0051] The surface of the leather material is divided into a grain surface and a flesh surface. The grain surface has a tight fiber structure and a smooth surface. The flesh surface is the reverse side of the leather, and the fiber bundles are loose and coarse. In addition, there are different fiber structures inside the leather. The fibers in the papillary layer are thin and loose, and the collagen fiber bundles in the reticular layer are thick, so the fiber pores are also of different sizes. To construct a conductive gradient on the leather, it is necessary to ensure that the size of the conductive material can penetrate into different fiber structures and evenly combine with the fibers layer by layer. As shown in Table 1, the use of conductive materials combined with collagen fibers can effectively reduce the resistance of the leather, and the resistance of the conductive leather flesh surface prepared in this embodiment is not much different from that of the grain surface, while the resistance of the carbon black / hydrotalcite leather flesh surface obtained by filtering the conductive carbon black from the leather flesh surface is relatively large. This conclusion can be drawn that the preparation method of the present invention draws on the leather tanning method, uses the isoelectric point of collagen fibers, adjusts the pH so that the conductive material and the collagen fibers have different electrical properties, and enables the conductive material to enter the tightly woven leather fibers and combine with them through physical mechanical and electrostatic effects. That is, the present invention can make the conductive materials such as hydrotalcite, carbon black, polypyrrole and the like evenly enter the leather collagen fibers, construct a continuous conductive network inside the leather, and make the leather as a whole have stable conductivity.
[0052] Example 2
[0053] This embodiment provides a method for preparing electromagnetic shielding leather with a conductive gradient structure.
[0054] 1. Preparation of hydrotalcite dielectric leather
[0055] 15g goatskin is put into a rotary drum, and 30mL of water and 2.1g of salt are added successively as body lotion. 1mol / L formic acid solution is used to adjust the pH of the body lotion in the rotary drum in small amounts and repeatedly until the pH of the body lotion is 2.5. The rotary drum is rotated for 30min, and the pickling treatment of the goatskin is completed. Then 2.4g of hydrotalcite is added into the rotary drum, and after rotating for 2h, 1mol / L of sodium bicarbonate solution is added to adjust the pH to 5.5, and the hydrotalcite is allowed to stand for 24h so that the collagen fibers of the goatskin are evenly combined to obtain hydrotalcite dielectric leather.
[0056] 2. Preparation of carbon black / hydrotalcite conductive leather
[0057] The hydrotalcite dielectric leather was placed in a 0.5 mol / L conductive carbon black aqueous solution, and the pH of the conductive carbon black aqueous solution was adjusted to 6 using a 1 mol / L sodium bicarbonate solution. After ultrasonic treatment for 15 minutes, the drum was rotated for 3 hours to combine the conductive carbon black with the collagen fibers through physical and mechanical action to obtain carbon black / hydrotalcite conductive leather.
[0058] 3. Preparation of polypyrrole / carbon black / hydrotalcite conductive leather
[0059] In an environment of 15°C, 0.5 mol / L of pyrrole monomer was dispersed in a mixed solution of 15 mL of ethanol and 15 mL of water to obtain a mixed solution. Carbon black / hydrotalcite conductive leather was placed in the mixed solution, the drum was rotated vigorously for 2 hours, 1 mol / L ferric chloride solution was added, and the drum was rotated slowly for 3 hours to obtain polypyrrole / carbon black / hydrotalcite conductive leather.
[0060] Example 3
[0061] This embodiment provides a method for preparing electromagnetic shielding leather with a conductive gradient structure.
[0062] 1. Preparation of hydrotalcite dielectric leather
[0063] 20g goat skin is put into a rotary drum, and then 40mL of water and 2.8g of salt are added successively as a body lotion. The pH of the body lotion in the rotary drum is adjusted repeatedly with a 1mol / L formic acid solution in small amounts until the pH of the body lotion is 3. The rotary drum is rotated for 30min, and the pickling treatment of the goat skin is completed. Then 2.8g of hydrotalcite is added into the rotary drum, and after rotating for 2h, a 1mol / L sodium bicarbonate solution is added to adjust the pH to 6, and the hydrotalcite is allowed to stand for 24h to uniformly combine with the collagen fibers of the goat skin to obtain a hydrotalcite dielectric leather.
[0064] 2. Preparation of carbon black / hydrotalcite conductive leather
[0065] The hydrotalcite dielectric leather was placed in a 1 mol / L conductive carbon black aqueous solution, and the pH of the conductive carbon black aqueous solution was adjusted to 7 using a 1 mol / L sodium bicarbonate solution. After ultrasonic treatment for 15 minutes, the drum was rotated for 4 hours to combine the conductive carbon black with the collagen fibers through physical and mechanical action to obtain the carbon black / hydrotalcite conductive leather.
[0066] 3. Preparation of polypyrrole / carbon black / hydrotalcite conductive leather
[0067] In an environment of 30°C, 0.5 mol / L of pyrrole monomer was dispersed in a mixed solution of 25 mL of ethanol and 25 mL of water to obtain a mixed solution. Carbon black / hydrotalcite conductive leather was placed in the mixed solution, the drum was rotated vigorously for 2 hours, 0.5 mol / L ferric chloride solution was added, and the drum was rotated slowly for 3 hours to obtain polypyrrole / carbon black / hydrotalcite conductive leather.
[0068] Example 4
[0069] This embodiment provides a method for preparing electromagnetic shielding leather with a conductive gradient structure.
[0070] 1. Preparation of hydrotalcite dielectric leather
[0071] 15g goat skin is put into a rotary drum, and 30mL of water and 2.1g of salt are added successively as body lotion. 1mol / L formic acid solution is used to adjust the pH of the body lotion in the rotary drum in small amounts and repeatedly until the pH of the body lotion is 3.5. The rotary drum is rotated for 30min, and the pickling treatment of the goat skin is completed. Then 2.4g of hydrotalcite is added into the rotary drum, and after rotating for 4h, 1mol / L of sodium bicarbonate solution is added to adjust the pH to 6, and the hydrotalcite is allowed to stand for 24h to uniformly combine the collagen fibers of the goat skin to obtain the hydrotalcite dielectric leather.
[0072] 2. Preparation of carbon black / hydrotalcite conductive leather
[0073] The hydrotalcite dielectric leather was placed in a 0.5 mol / L conductive carbon black aqueous solution, and the pH of the conductive carbon black aqueous solution was adjusted to 6 using a 1 mol / L sodium bicarbonate solution. After ultrasonic treatment for 15 minutes, the drum was rotated for 4 hours to combine the conductive carbon black with the collagen fibers through physical and mechanical action to obtain carbon black / hydrotalcite conductive leather.
[0074] 3. Preparation of polypyrrole / carbon black / hydrotalcite conductive leather
[0075] In an environment of 5°C, 1 mol / L pyrrole monomer was dispersed in a mixed solution of 15 mL ethanol and 15 mL water to obtain a mixed solution. Carbon black / hydrotalcite conductive leather was placed in the mixed solution, the drum was rotated vigorously for 2 hours, 1 mol / L ferric chloride solution was added, and the drum was slowly rotated for 6 hours to obtain polypyrrole / carbon black / hydrotalcite conductive leather.
[0076] The embodiments described above are part of the embodiments of the present invention, but not all of them. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but only represents selected embodiments of the present invention. All other embodiments obtained without creative work and related deductions and substitutions made by ordinary technicians in the field under the conditions of the concept of the present invention belong to the scope of protection of the present invention.
Claims
1. A method for preparing leather having a conductive gradient structure, characterized in that: include: adding a dielectric material with wave-absorbing properties to the pre-treated acid leather bath solution for a first impregnation treatment to obtain dielectric leather; placing the dielectric leather in a solution containing a conductive material for a second dipping treatment to obtain conductive leather; The conductive leather is placed in a solution containing polymer monomers for a third immersion treatment, and an oxidant is added to carry out polymerization reaction to obtain leather with a conductive gradient structure.
2. The method for preparing leather having a conductive gradient structure according to claim 1, wherein: The pretreatment is pickling treatment; The pH of the bath in the pickling treatment is 2.5 to 3.
5.
3. The method for preparing leather having a conductive gradient structure according to claim 1, wherein: The dielectric material with wave absorbing properties is hydrotalcite; The mass of the hydrotalcite is 5% to 10% of the mass of water.
4. The method for preparing leather having a conductive gradient structure according to claim 1, wherein: The first immersion treatment includes: rotating, adjusting pH, and standing; The pH is adjusted to 4-6; The rotation time is 2 to 4 hours; The standing time is 6 to 24 hours.
5. The method for preparing leather having a conductive gradient structure according to claim 1, wherein: The conductive material is carbon black.
6. The method for preparing leather having a conductive gradient structure according to claim 1, characterized in that: The second immersion treatment includes: adjusting pH, ultrasonication, and rotation; The pH is adjusted to 5.5-7; The ultrasonic time is 15 minutes; The rotation time is 2 to 6 hours.
7. The method for preparing leather having a conductive gradient structure according to claim 1, characterized in that: The polymer monomer is pyrrole, and the oxidant is ferric chloride.
8. The method for preparing leather having a conductive gradient structure according to claim 1, characterized in that: The third dipping process includes: rotating; The rotation time is 1 to 2 hours.
9. Leather with a conductive gradient structure prepared by the method for preparing leather with a conductive gradient structure according to any one of claims 1 to 8.
10. Use of the leather with a conductive gradient structure as claimed in claim 9 in preparing electromagnetic shielding materials.
Citation Information
Patent Citations
Leather with electromagnetic shielding performance and preparing method thereof
CN105219895A
Conductive leather and preparation method thereof
CN110957058A
Chromium-containing wastewater treatment method and application thereof in preparation of electromagnetic shielding leather
CN117303553A
Electromagnetic shielding material and method for manufacturing the same
JP2005311039A