Cast aluminum alloy refining modifier and preparation method thereof

By using a combination of Ti, B, Sr and P elements to refine the deteriorating agent, combined with argon and powder refining technology, the problems of poor refining and deterioration effect and low cleanliness of cast aluminum alloys in the prior art are solved, and casting is achieved The high fluidity, strength and plasticity of aluminum alloys meet the production needs of high clean and high performance.

CN119061271APending Publication Date: 2024-12-03GUANGDONG ENG POLYTECHNIC COLLEGE +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410995654.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing cast aluminum alloy refinement agents cannot completely eliminate coarse dendritic α-Al grains and coarse needle-shaped or sheet-like eutectic Si phases, primary Si phases and Fe-rich phases, resulting in poor fluidity, strength and It has low plasticity and low cleanliness, making it difficult to meet the production needs of high strength, high plasticity and high cleanliness.

Method used

Using a refinement agent of Ti 4.8-5.2%, B 2.4-2.8%, Sr 0.5-1.5%, P 0.05-0.15%, α-Al grains and eutectics are refined by forming TiB2 particles and Sr elements. The Si phase and the primary crystal Si phase, the Fe-rich phase of trace B elements are refined, combined with the spray refining technology of argon and powder refining agents, to improve the fluidity and tissue uniformity of aluminum alloys and reduce the content of gas slag.

Benefits of technology

The deep refinement and deterioration of α-Al grains, eutectic Si phases, primary Si phases and Fe-rich phases in cast aluminum alloys is achieved, which improves the fluidity, strength and plasticity of cast aluminum alloys, and meets high cleanliness and high performance. The production demand has significantly reduced the gas slag content and impurity element content of aluminum alloy liquid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061271A_ABST
    Figure CN119061271A_ABST
Patent Text Reader

Abstract

The invention discloses a refining modifier for a cast aluminum alloy and a preparation method of the refining modifier. The refining modifier is prepared from the following components in percentage by mass: 4.8 to 5.2 percent of Ti, 2.4 to 2.8 percent of B, 0.5 to 1.5 percent of Sr, 0.05 to 0.15 percent of P, less than or equal to 0.15 percent of Fe and the balance of Al and inevitable impurities. The preparation method comprises the following steps: burdening, melting an aluminum ingot, adding raw materials to react to obtain an aluminum alloy liquid, blowing, refining, deslagging and degassing, and casting to form an ingot. The problems that a traditional refining modifier is unstable in effect, single in function, low in cleanliness and the like are solved, deep refining modification of alpha-Al grains, an eutectic Si phase, a primary Si phase and a Fe-rich phase in the cast aluminum alloy is achieved, harm of the coarse alpha-Al grains, the Si phase and the Fe-rich phase is eliminated, the casting fluidity and mechanical performance of the aluminum alloy are improved, and the casting quality of the cast aluminum alloy is improved. And the production requirements of high-toughness and high-cleanliness cast aluminum alloy parts are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of casting aluminum alloy preparation, and in particular relates to a casting aluminum alloy refining modifier and a preparation method thereof. Background Art

[0002] Cast aluminum alloy is an aluminum alloy with aluminum and silicon as the main elements. It has good casting performance, corrosion resistance and mechanical properties. It is widely used in metal mold gravity casting, squeeze casting, low-pressure casting and high-pressure die casting, etc., and is used to cast various aluminum alloy parts. The performance of cast aluminum alloy is closely related to its organizational state, including the morphology and size of α-Al grains, eutectic Si phase, primary Si phase and Fe-rich phase. Without refinement and modification, the α-Al grains in cast aluminum alloys are usually coarse dendrites, and the eutectic Si phase, primary Si phase and Fe-rich phase are usually coarse needles or flakes. Coarse dendritic α-Al grains will reduce the casting fluidity of aluminum alloys, resulting in incomplete filling of cast aluminum alloy parts, and defects such as shrinkage cavities and looseness inside. Coarse needle-shaped or flake eutectic Si phase, primary Si phase and Fe-rich phase will split the matrix of cast aluminum alloy, destroy the continuity of the organization, cause local stress concentration, become the crack source and crack propagation direction of cast aluminum alloy parts, and reduce the strength and plasticity of cast aluminum alloy parts. Therefore, refining modifiers must be added during the smelting process of cast aluminum alloys for refining and modification.

[0003] Patent document with publication number CN117867305A discloses a method for controlling the microstructure of an integrated die-casting Al-Si alloy with high elongation, comprising first adding an Al-Ti-B master alloy containing a specific titanium-boron ratio into a die-casting Al-Si alloy, causing it to completely melt in a short time through an auxiliary process, then quickly adding an Al-Sr master alloy for smelting and modification, and finally die-casting to obtain an integrated die-casting Al-Si alloy with high elongation.

[0004] Patent document with publication number CN116287836A discloses a composite refining modifier for cast aluminum-silicon alloy, which uses Al-10Sr, Al-10Y master alloy and titanium agent as the composite refining modifier, the addition ratio of Sr is 0.01-0.05% of the total mass of the aluminum alloy, the addition ratio of Y is 0.1-0.5% of the total mass of the aluminum alloy, and the addition ratio of Ti is 0.01-0.15% of the total mass of the aluminum alloy.

[0005] The patent document with publication number CN110396615A discloses a multi-component aluminum-silicon alloy graded refinement and modification process, in which Al-4Zr master alloy, Al-10Sr master alloy and Al-10RE master alloy are added in three stages in sequence, which not only refines the grains of the multi-component aluminum-silicon alloy, but also significantly improves the precipitation morphology of the Si phase, Al2Cu phase and primary Fe-rich phase, thereby improving the strength of the cast multi-component aluminum-silicon alloy while significantly improving its plasticity.

[0006] Patent document with publication number CN115896552A discloses an alloy additive and a method for refining and modifying an Al-Si alloy, wherein the alloy additive includes Al-3Ti-4.35La and Al-5Ti-C; the mass ratio of Al-3Ti-4.35La to Al-5Ti-C is 1:1-5. The method for refining and modifying an Al-Si alloy includes melting an Al-Si alloy, mixing the alloy liquid and the refining modifier and then casting, and improving the mechanical properties of the Al-Si alloy by reducing the size of the α-A1 phase and the eutectic silicon phase in the Al-Si alloy.

[0007] Patent document with publication number CN115522103A discloses a new type of refining modifier for hypoeutectic aluminum-silicon alloy and its preparation and application method. The refining modifier is a new type of Al-Sr-Y-Sn refining modifier, and its components are composed of Sr 2.5-4%, Y 7-8.5%, Sn 0.1-2% by mass percentage, and the balance is Al. It has the integrated function of modification and refining, and effectively reduces the tendency of alloy melt to get air.

[0008] Patent document with publication number CN112921204A discloses a composite refining modifier for recycled aluminum-silicon alloy and a preparation method thereof. The composite refining modifier is composed of the following components in mass percentage: Ti 3.8-4.2%, Ni 0.9-1.1%, Ba 0.8-1.2%, C 0.7-0.9%, B 0.4-0.6%, Fe≤0.15%, and the balance is Al and other inevitable impurity elements, which solves the problems of traditional refining modifiers such as easy poisoning by Si, unstable effect, and pores generated by hydrogen absorption.

[0009] According to the results of literature retrieval and production practice experience, the existing casting aluminum alloy refining and modification agents still have one or more of the following problems: (1) The refining and modification effect is still poor, and it is difficult to completely eliminate the coarse dendritic α-Al grains and the coarse needle-shaped or lamellar eutectic Si phase, primary Si phase and Fe-rich phase, which makes it difficult to meet the production needs of high-strength and high-plasticity casting aluminum alloys. (2) The refining and modification function is single, and it is impossible to simultaneously achieve the refining and modification of α-Al grains, eutectic Si phase, primary Si phase and Fe-rich phase in the casting aluminum alloy. (3) The cleanliness is low and the gas slag content is high, which causes secondary pollution to the casting aluminum alloy liquid and cannot meet the production needs of high-cleanliness casting aluminum alloys. Summary of the invention

[0010] In view of the problems and shortcomings mentioned in the background technology, the present invention provides a refining and modifying agent for cast aluminum alloy and a preparation method thereof. By scientifically designing the component composition of the refining and modifying agent and optimizing the preparation method of the refining and modifying agent, the refining and modifying effect and cleanliness of the refining and modifying agent are improved, and deep refining and modifying of α-Al grains, eutectic Si phase, primary Si phase and Fe-rich phase in the cast aluminum alloy are achieved, and the harm of coarse dendritic α-Al grains and coarse needle-shaped or flaky eutectic Si phase, primary Si phase and Fe-rich phase to the fluidity, strength and plasticity of the cast aluminum alloy is eliminated, thereby meeting the production requirements of high-cleanliness and high-performance cast aluminum alloy.

[0011] The technical solution adopted by the present invention to achieve the above-mentioned purpose is as follows:

[0012] The first aspect of the present invention provides a casting aluminum alloy refining and modifier, which is characterized in that the refining and modifier is composed of the following components in mass percentage: Ti 4.8-5.2%, B 2.4-2.8%, Sr0.5-1.5%, P 0.05-0.15%, Fe≤0.15%, and the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.15%.

[0013] Among them, the main role of Ti element is to refine α-Al grains. Ti element can form TiB2 particles with B element, and TiB2 particles can act as heterogeneous nucleation cores of α-Al grains. During the solidification process of cast aluminum alloy liquid, a large number of TiB2 particles increase the number of heterogeneous nucleation cores of α-Al grains, thereby refining α-Al grains, transforming α-Al grains from coarse dendrites to fine particles or spheres, improving the fluidity of cast aluminum alloys, and improving the uniformity of the organizational composition of cast aluminum alloys.

[0014] The role of B element is first to form TiB2 particles with Ti element, which plays a role in refining α-Al grains. Secondly, it refines and modifies the Fe-rich phase. Fe element is an inevitable impurity element in cast aluminum alloy. It usually exists in the form of coarse needle-shaped or flake-shaped Fe-rich phases such as FeAl3 and FeSiAl3, which becomes the crack source and crack extension direction of the cast aluminum alloy fracture, reducing the strength and plasticity of the cast aluminum alloy. Trace amounts of B element can transform the Fe-rich phase from coarse needle-shaped to fine particles and dispersed in the cast aluminum alloy, which can not only eliminate the harm of coarse Fe-rich phase, but also enhance the strength of the cast aluminum alloy. The mass ratio of B to Ti element in TiB2 particles is 0.45. In order to enable B element to form a sufficient number of TiB2 particles with Ti element and to have enough B element to refine and modify the Fe-rich phase, the mass ratio of B element to Ti element is required to be greater than 0.45. As a preferred embodiment, the mass percentage of B element to Ti element satisfies: B>Ti×0.45+0.2.

[0015] The main function of Sr element is to refine and modify eutectic Si. Si element is the main alloying element of cast aluminum alloy, and improves the fluidity of cast aluminum alloy by forming Al+Si eutectic liquid phase with Al. However, eutectic Si phase usually exists in coarse needle-like form in cast aluminum alloy. Since Si phase is a hard and brittle phase, it will not only split the matrix of cast aluminum alloy, but also cause local stress concentration, becoming the crack source and crack propagation direction of cast aluminum alloy fracture, which will not only reduce the strength of cast aluminum alloy, but also seriously reduce the plasticity of cast aluminum alloy. Sr element has a good refining and modifying effect on eutectic Si phase, which can transform the morphology of eutectic Si phase from coarse needle-like to fine granular or short fiber-like, thereby eliminating the damage of coarse needle-like eutectic Si phase to the strength and plasticity of cast aluminum alloy, and improving the strength and plasticity of cast aluminum alloy.

[0016] The main function of the P element is to refine and modify the primary Si phase. In addition to forming the eutectic Si phase, the Si element in the cast aluminum alloy will also form a coarse block primary Si phase, especially for the hypereutectic cast aluminum alloy with a high Si content, a large amount of coarse crystal Si phase will be formed. The primary Si phase is also a hard and brittle phase, which not only splits the cast aluminum alloy matrix, but also causes local stress concentration, becomes the crack source and crack propagation direction of the cast aluminum alloy fracture, and reduces the strength and plasticity of the cast aluminum alloy. The P element has a good refining and metamorphic effect on the primary Si phase, which can transform the primary Si phase from a coarse block to a fine granular state and dispersedly distribute it in the cast aluminum alloy matrix, which can not only eliminate the harm of the coarse block primary Si phase to the strength and plasticity of the cast aluminum alloy, but also improve the wear resistance of the cast aluminum alloy.

[0017] Fe and other impurity elements are inevitable in the refining modifier. In order to avoid adding the refining modifier to increase the content of impurity elements in the cast aluminum alloy, the content of impurity elements in the refining modifier must be strictly controlled. Preferably, the content of impurity element Fe is ≤0.15%, the content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.15%.

[0018] The second aspect of the present invention provides a method for preparing a casting aluminum alloy refinement modifier, which is characterized by comprising the following steps in sequence:

[0019] Step 1: According to the composition and mass percentage of the refined modifier, aluminum ingot, strontium ingot, aluminum-phosphorus alloy, potassium fluorotitanate and potassium fluoroborate are selected as raw materials for batching;

[0020] Step 2: Heat the aluminum ingot and melt it into aluminum liquid;

[0021] Step 3: adding potassium fluorotitanate and potassium fluoroborate to the aluminum liquid, stirring and reacting to obtain aluminum alloy liquid;

[0022] Step 4: adding strontium ingot and aluminum-phosphorus alloy into aluminum alloy liquid, stirring and melting into aluminum alloy liquid;

[0023] Step 5: using argon gas and powder refining agent to spray, refine, remove slag and degas the aluminum alloy liquid;

[0024] Step 6: Use mixed gas to spray, refine, remove slag and degas the aluminum alloy liquid;

[0025] Step seven: Casting the aluminum alloy liquid into an aluminum alloy ingot to obtain the cast aluminum alloy refining modifier.

[0026] Furthermore, the aluminum content of the aluminum ingot in step 1 is ≥ 99.7%, and the strontium content of the strontium ingot is

[0027] ≥99.9%, the phosphorus content of the aluminum-phosphorus alloy is 5%, the purity of potassium fluorotitanate is ≥99.5%, and the purity of potassium fluoroborate is ≥99.5%. The purity of the raw materials will directly affect the purity of the refining modifier. In order to avoid the pollution of the cast aluminum alloy caused by the addition of refining modifiers and reduce the purity of the cast aluminum alloy, the purity of the raw materials must be appropriately limited. The higher the purity of the raw materials, the higher the purity of the prepared refining modifier, but the higher the purity of the raw materials, the higher the price of the raw materials, and the corresponding increase in the production cost of the refining modifier. Preferably, an aluminum ingot with an aluminum content of 99.7%, a strontium ingot with a strontium content of 99.9%, and potassium fluorotitanate and potassium fluoroborate with a purity of 99.5% are selected.

[0028] Furthermore, the heating and melting temperature of the aluminum ingot in step 2 is 740-760°C. The heating and melting of the aluminum ingot must be carried out at a certain superheated temperature. If the heating and melting temperature is too low, the aluminum ingot is difficult to melt or the melting speed is slow, which affects the production efficiency. However, the heating and melting temperature of the aluminum ingot should not be too high, otherwise it will aggravate the oxidation and burning of the aluminum ingot and the aluminum liquid, and increase the production cost.

[0029] Furthermore, the stirring reaction time described in step 3 is 30-60 minutes. In order to promote the reaction of potassium fluorotitanate and potassium fluoroborate to form TiB2 particles, stirring must be performed, and the stirring reaction time cannot be less than 30 minutes, so that potassium fluorotitanate and potassium fluoroborate have sufficient reaction time. However, the stirring reaction time should not exceed 60 minutes, otherwise it will aggravate the oxidation and burning of the aluminum liquid. After the stirring reaction is completed, the scum on the surface of the aluminum alloy liquid should be promptly scraped off, and a covering agent should be sprinkled on the surface of the aluminum alloy liquid to prevent the oxidation and burning of the aluminum alloy liquid.

[0030] Furthermore, in step 4, the strontium ingot is coated with aluminum foil for protection before being added to the aluminum alloy liquid. Since metal strontium has active chemical properties, it is easy to oxidize and burn at high temperatures. In order to avoid oxidation and burning of the strontium ingot when it contacts the high-temperature aluminum liquid and improve the recovery rate of metal strontium, the strontium ingot is coated with aluminum foil for protection before being added to the aluminum alloy liquid to avoid oxidation and burning of the strontium ingot.

[0031] Furthermore, the purity of the argon gas in step five is ≥99.99%, the amount of the powder refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, the temperature of the aluminum alloy liquid during spray refining is 700-720°C, and the spray refining time is 10-20 minutes.

[0032] Adding a refining modifier to the casting aluminum alloy liquid, the purity of the refining modifier will directly affect the purity of the casting aluminum alloy liquid. Since the surface of the raw materials for preparing the refining modifier inevitably carries oxides, dust and water vapor, especially the addition of potassium fluorotitanate and potassium fluoroborate, the refining modifier aluminum alloy liquid contains a large amount of inclusions and entrapped gas, the gas is mainly hydrogen. If these inclusions and hydrogen are not removed as much as possible, it will eventually cause pollution to the casting aluminum alloy liquid, reduce the purity of the casting aluminum alloy liquid, and finally deteriorate the mechanical properties of the casting aluminum alloy.

[0033] The spray refining adopts a powder spraying tank and a stainless steel pipe, and uses argon as a carrier to spray the powdered refining agent into the refining and modifying agent aluminum alloy liquid, so that the powdered refining agent contacts and reacts with the aluminum alloy liquid, and then the inclusions and hydrogen in the aluminum alloy liquid are taken out of the aluminum alloy liquid. The deslagging and degassing effect of spray refining is related to the purity of argon, the amount of refining agent, the temperature of the aluminum alloy liquid and the spray refining time. The higher the purity of argon, the greater the amount of refining agent, the longer the spray refining time, the better the effect of deslagging and dehydrogenation, but the production cost will also increase accordingly. If the spray refining makes the temperature of the aluminum alloy liquid too high or the spray refining time is too long, the oxidation and burning of the aluminum alloy liquid will also increase. After the spray refining is completed and the scum on the surface of the aluminum alloy liquid is scraped off, the aluminum alloy liquid needs to be allowed to stand for a period of time so that the inclusions and bubbles in the aluminum alloy liquid have sufficient time to escape. The standing time of the aluminum alloy liquid is not less than 30 minutes, and preferably the standing time of the aluminum alloy liquid is 30-40 minutes.

[0034] Furthermore, the powder refining agent in step five is composed of the following components in mass percentage: NaCl 35.12%, NaF 19.84%, TiCl 3 16.51%, SrSO 4 10.06%, KPO 3 11.45%, and Na 2 B 4 O 77.02%.

[0035] The deslagging and dehydrogenation effect of powder spray refining is closely related to the composition of the refining agent. The existing refining agent is mainly obtained by crushing and mixing fluoride salt and chloride salt, which leads to a high melting point of the refining agent, low deslagging and dehydrogenation efficiency, and also causes the loss of Ti, B, Sr and P elements in the aluminum alloy liquid of the refining agent, affecting the effect of the refining agent, and cannot meet the production needs of high-cleanliness and high-efficiency refining agent. In order to solve the problems and shortcomings of the existing refining agent, the present invention has developed a new powder refining agent, in which NaCl reacts with the aluminum alloy liquid to generate AlCl3 with a boiling point of only 180°C. The AlCl3 bubbles absorb and capture inclusions and hydrogen in the aluminum alloy liquid during the floating process, and then escape from the aluminum alloy liquid together, playing a role in deslagging and dehydrogenation. The main function of NaF is to destroy the aluminum oxide film by forming molten salt, so that inclusions such as aluminum oxide are dissolved in the molten salt, increase the surface tension between the inclusions and the aluminum alloy liquid, promote the separation of inclusions such as aluminum oxide from the aluminum alloy liquid, and enhance the deslagging function of the refining agent. TiCl3 reacts with aluminum alloy liquid to generate AlCl3 bubbles, which absorb and capture inclusions and hydrogen in the aluminum alloy liquid during the floating process, thereby enhancing the slag and hydrogen removal capabilities of the refining agent. The Ti element obtained by the reaction can supplement the Ti content of the aluminum alloy liquid. SrSO4 reacts with aluminum alloy liquid to generate SO2 bubbles, which absorb and capture inclusions and hydrogen in the aluminum alloy liquid during the floating process, thereby enhancing the slag and hydrogen removal capabilities of the refining agent. The Sr element obtained by the reaction can supplement the Sr content of the aluminum alloy liquid. KPO3 reacts with aluminum alloy liquid to generate P elements, which can supplement the P content of the aluminum alloy liquid and enhance the refining and modification function of the refining modifier. Na2B4O7 reacts with aluminum liquid to generate B elements, which can supplement the B content of the aluminum alloy liquid, thereby enhancing the refining and modification function of the refining modifier on the coarse Fe-rich phase and the refining and modification function of the refining modifier.

[0036] Furthermore, the preparation method of the powder refining agent described in step five comprises the following steps in sequence: (1) according to the composition and mass percentage of the powder refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of ≥99.8% are selected as raw materials for batching; (2) the ingredients are added into water at a temperature of 70°C and stirred to dissolve into an aqueous solution, the mass ratio of water to ingredients being 1.2, and then the aqueous solution is heated to 100°C to evaporate to obtain solid crystals; (3) the solid crystals are crushed into powder with a particle size of less than 2 mm, and the powder is dried and dehydrated at 160°C for 4 hours to obtain the powder refining agent.

[0037] The deslagging and dehydrogenation effect of the refining agent is closely related to its preparation method. Existing refining agents are usually obtained by directly mixing chloride salts and fluoride salts after mechanical crushing. The components of this refining agent exist independently of each other, resulting in a high melting point of the refining agent, a lack of synergy between the components, and low deslagging and dehydrogenation efficiency of the refining agent. The present invention breaks through the traditional preparation method and adopts a solution evaporation method to prepare the refining agent. Through solution evaporation, the components are re-solidified and recrystallized to form a eutectic with a lower melting point. For example, the melting point of NaCl is usually 801°C, and the melting point of NaF is usually 993°C. When the two form a NaCl·NaF eutectic, the melting point drops to 698°C, thereby greatly reducing the melting point of the refining agent, making the refining agent easier to dissolve in the aluminum alloy liquid of the refining modifier, and playing a synergistic role during refining, which can significantly enhance the deslagging and dehydrogenation ability of the refining agent and improve the purity of the refining modifier.

[0038] Furthermore, the amount of the mixed gas in step 6 is 2-3 cubic meters per ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.3-0.5×10 5 Pa, the temperature of the aluminum alloy liquid during spray refining is 700-720℃, and the spray refining time is 10-15 minutes.

[0039] After powder spray refining, the gas slag content of aluminum alloy liquid has been greatly reduced, but the aluminum alloy liquid still contains gas slag, because the powder refining agent refining process re-introduces inclusions such as chloride salts and fluoride salts. In addition, although the powder refining agent spray refining also has a dehydrogenation effect, the dehydrogenation effect is limited. The reason is that the powder refining agent inevitably contains water, which will also be introduced during the spray refining dehydrogenation, causing the aluminum alloy liquid to absorb hydrogen again, so that the dehydrogenation of the powder refining agent spray refining is always in a dynamic equilibrium process. It is difficult for the powder refining agent spray refining to reduce the hydrogen content of the aluminum alloy liquid to below 0.2ml / 100gAl. Therefore, in order to obtain a highly clean aluminum alloy liquid, refining, dehydrogenation and deslag removal are also necessary.

[0040] The mixed gas injection refining adopts a stainless steel pipe or a degasser to inject the mixed gas into the aluminum alloy liquid, so that the mixed gas forms fine bubbles that contact and react with the aluminum alloy liquid, and the hydrogen and inclusions in the aluminum alloy liquid are brought out of the liquid surface by the floating of the bubbles, so as to achieve the purpose of deep slag removal and hydrogen removal.

[0041] The dehydrogenation and slag removal effect of mixed gas spray refining is related to the amount of mixed gas used, the temperature of the aluminum alloy liquid and the spray refining time. The greater the amount of mixed gas used, the longer the spray refining time, and the better the deslagging and dehydrogenation effect of the spray refining, but the production cost will also increase accordingly. If the temperature of the aluminum alloy liquid is too high or the spray refining time is too long, the oxidation and burning of the aluminum alloy liquid will also increase. After the spray refining is completed and the scum on the surface of the aluminum alloy liquid is removed, a covering agent should be sprinkled on the surface of the aluminum alloy liquid in time to avoid oxidation and burning of the aluminum alloy liquid and hydrogen absorption. After sprinkling the covering agent, the aluminum alloy liquid needs to be left to stand for a period of time so that the bubbles in the aluminum alloy liquid have sufficient time to escape. The standing time of the aluminum alloy liquid cannot be less than 20 minutes. Preferably, the standing time of the aluminum alloy liquid is 20-30 minutes.

[0042] Furthermore, the mixed gas in step six is ​​composed of argon gas with a purity of ≥99.99%, sulfur hexafluoride and carbon monoxide, the volume percentage of sulfur hexafluoride in the mixed gas is 9-11%, and the volume percentage of carbon monoxide is 3-5%.

[0043] In the existing gas injection refining technology, inert gas nitrogen or argon, or a mixture of inert gas and chlorine, is usually injected into the aluminum alloy liquid. The relative molecular mass of nitrogen is 28.01 and the density is 1.25kg / m 3 The relative molecular mass of argon is 39.94 and the density is 1.78 kg / m 3 The relative molecular mass of chlorine is 70.91 and the density is 3.21kg / m 3 . Due to the small relative molecular mass and low density of nitrogen, argon and chlorine, the bubbles float up faster in the aluminum alloy liquid, and the contact time between the bubbles and the aluminum alloy liquid is shorter, which limits the time for the bubbles to capture and adsorb hydrogen and inclusions, greatly affecting the dehydrogenation and deslagging effect of gas injection refining. In addition, although the relative density of chlorine is relatively large, chlorine is a toxic gas with a strong pungent odor, which will not only seriously corrode the smelting furnace and smelting tools, but also cause serious environmental pollution.

[0044] Aiming at the problems and shortcomings of the existing gas injection refining technology, in order to improve the dehydrogenation and slag removal effect of gas injection refining, the present invention injects a mixed gas consisting of argon with a purity of ≥99.99%, sulfur hexafluoride with a purity of ≥99.99% and carbon monoxide with a purity of ≥99.99% into the aluminum alloy liquid, wherein sulfur hexafluoride is a high-density and high-stability gas with a relative molecular mass of 146.05 and a density of 6.5kg / m 3, and sulfur hexafluoride is non-toxic, non-flammable and non-corrosive. Adding 9-11% by volume of sulfur hexafluoride to the mixed gas can significantly slow down the floating speed of bubbles in the aluminum alloy liquid, increase the contact time between the bubbles and the aluminum alloy liquid, and enable the bubbles to capture and absorb more hydrogen and inclusions, thereby improving the dehydrogenation and deslagging effect of gas injection refining. Adding 3-5% by volume of carbon monoxide to the mixed gas is to allow carbon monoxide to capture oxygen in the aluminum alloy liquid to form carbon dioxide, prevent oxygen from forming an aluminum oxide film on the surface of the bubble again with aluminum, enhance the ability of the bubbles to capture and absorb hydrogen and inclusions, and improve the deslagging and dehydrogenation effect of gas injection refining. Through mixed gas injection refining, the hydrogen content of the aluminum alloy liquid can be reduced to below 0.13ml / 100gAl, and the inclusion content can be reduced to 0.08mm 2 / kgAl or less, thereby greatly improving the cleanliness of the aluminum alloy liquid.

[0045] Furthermore, in step 7, when the aluminum alloy liquid is cast into an aluminum alloy ingot, the pouring temperature of the aluminum alloy liquid is 680-700°C. The pouring temperature of the aluminum alloy liquid cannot be lower than 680°C, otherwise it is easy to cause cold shut defects on the surface of the aluminum alloy ingot, affecting the surface quality of the aluminum alloy ingot. However, the pouring temperature of the aluminum alloy liquid should not be too high, otherwise it will increase the solidification cooling time of the aluminum alloy liquid and reduce production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The present invention will be further described below in conjunction with the accompanying drawings.

[0047] Figure 1 The microstructure x100 image of the ADC10 cast aluminum alloy ingot after refinement and modification in Example 6;

[0048] Figure 2 This is the x100 image of the microstructure of the ADC10 cast aluminum alloy ingot before refinement and modification in Example 6. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] Example 1

[0051] The casting aluminum alloy refining modifier is composed of the following components in mass percentage: Ti 5.0%, B 2.5%, Sr0.9%, P 0.11%, Fe≤0.15%, the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.15%. The preparation method comprises the following steps in sequence: step 1: according to the composition and mass percentage of the refining modifier, an aluminum ingot with an aluminum content of 99.7%, a strontium ingot with a strontium content of 99.9%, an aluminum-phosphorus alloy with a phosphorus content of 5%, potassium fluorotitanate with a purity of 99.5% and potassium fluoroborate with a purity of 99.5% are selected as raw materials for batching; step 2: heating the aluminum ingot at 750°C to melt it into aluminum liquid; step 3: adding potassium fluorotitanate and potassium fluoroborate to the aluminum liquid, stirring and reacting for 45 minutes to obtain an aluminum alloy liquid; step 4: using aluminum foil to Strontium ingot coating, adding strontium ingot and aluminum phosphorus alloy to aluminum alloy liquid, stirring and melting into aluminum alloy liquid; step five: using argon gas with a purity of 99.99% and a powder refining agent with a weight of 0.15% of the aluminum alloy liquid to spray and refine the aluminum alloy liquid at 710°C for 15 minutes to remove slag and degassing, scrape off the scum on the surface of the aluminum alloy liquid, and let the aluminum alloy liquid stand for 35 minutes; step six: using a mixed gas composed of argon gas with a purity of 99.99%, sulfur hexafluoride and carbon monoxide to spray and refine the aluminum alloy liquid at 710°C for 12 minutes to remove slag and degassing, scrape off the scum on the surface of the aluminum alloy liquid, and let the aluminum alloy liquid stand for 25 minutes, the amount of the mixed gas is 2.5 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.4×10 5 Pa; Step seven: casting the aluminum alloy liquid into an aluminum alloy ingot at 690° C. to obtain the cast aluminum alloy refining modifier.

[0052] Example 2

[0053] The casting aluminum alloy refinement modifier is composed of the following components in mass percentage: Ti 5.2%, B

[0054] 2.8%, Sr 0.5%, P 0.15%, Fe≤0.15%, the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.15%. The preparation method comprises the following steps in sequence: Step 1: According to the composition and mass percentage of the refining modifier, an aluminum ingot with an aluminum content of 99.7%, a strontium ingot with a strontium content of 99.9%, an aluminum-phosphorus alloy with a phosphorus content of 5%, potassium fluorotitanate with a purity of 99.5%, and potassium fluoroborate with a purity of 99.5% are selected as raw materials for batching; Step 2: The aluminum ingot is heated and melted at 760°C to form aluminum liquid; Step 3: Potassium fluorotitanate and potassium fluoroborate are added to the aluminum liquid, and the reaction is stirred for 30 minutes to obtain an aluminum alloy liquid; Step 4: Use aluminum foil to The strontium ingot is coated, and the strontium ingot and the aluminum phosphorus alloy are added to the aluminum alloy liquid, and the aluminum alloy liquid is stirred and melted into the aluminum alloy liquid; Step 5: The aluminum alloy liquid at 720°C is sprayed and refined for 20 minutes with argon gas with a purity of 99.99% and a powder refining agent with a weight of 0.1% of the aluminum alloy liquid, and the slag on the surface of the aluminum alloy liquid is scraped off, and the aluminum alloy liquid is allowed to stand for 30 minutes; Step 6: The aluminum alloy liquid at 720°C is sprayed and refined for 10 minutes with a mixed gas composed of argon gas with a purity of 99.99%, sulfur hexafluoride and carbon monoxide, and the slag on the surface of the aluminum alloy liquid is scraped off, and the aluminum alloy liquid is allowed to stand for 30 minutes. The amount of the mixed gas is 2 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.5×10 5 Pa; Step seven: casting the aluminum alloy liquid into an aluminum alloy ingot at 700° C. to obtain the cast aluminum alloy refining modifier.

[0055] Example 3

[0056] The casting aluminum alloy refinement modifier is composed of the following components in mass percentage: Ti 4.8%, B

[0057] 2.4%, Sr 1.5%, P 0.05%, Fe≤0.15%, the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.15%. The preparation method comprises the following steps in sequence: Step 1: According to the composition and mass percentage of the refining modifier, an aluminum ingot with an aluminum content of 99.7%, a strontium ingot with a strontium content of 99.9%, an aluminum-phosphorus alloy with a phosphorus content of 5%, potassium fluorotitanate with a purity of 99.5%, and potassium fluoroborate with a purity of 99.5% are selected as raw materials for batching; Step 2: The aluminum ingot is heated and melted at 740°C to form aluminum liquid; Step 3: Potassium fluorotitanate and potassium fluoroborate are added to the aluminum liquid, and the reaction is stirred for 60 minutes to obtain an aluminum alloy liquid; Step 4: Use aluminum foil to The strontium ingot is coated, and the strontium ingot and the aluminum phosphorus alloy are added to the aluminum alloy liquid, and the aluminum alloy liquid is stirred and melted into the aluminum alloy liquid; Step 5: The aluminum alloy liquid at 700°C is sprayed and refined for 20 minutes with argon gas with a purity of 99.99% and a powder refining agent with a weight of 0.2% of the aluminum alloy liquid, and the slag on the surface of the aluminum alloy liquid is scraped off, and the aluminum alloy liquid is allowed to stand for 40 minutes; Step 6: The aluminum alloy liquid at 700°C is sprayed and refined for 15 minutes with a mixed gas composed of argon gas with a purity of 99.99%, sulfur hexafluoride and carbon monoxide, and the slag on the surface of the aluminum alloy liquid is scraped off, and the aluminum alloy liquid is allowed to stand for 20 minutes. The amount of the mixed gas is 3 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.3×10 5 Pa; Step seven: casting the aluminum alloy liquid into an aluminum alloy ingot at 680° C. to obtain the cast aluminum alloy refining modifier.

[0058] Example 4

[0059] In this embodiment, the powder refining agent described in step 5 of embodiment 1-3 is prepared. The powder refining agent is composed of the following components in mass percentage: NaCl 35.12%, NaF 19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%. The preparation method comprises the following steps in sequence: (1) according to the composition and mass percentage of the powder refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of ≥99.8% are selected as raw materials for batching; (2) the ingredients are added into water at a temperature of 70° C. and stirred to dissolve into an aqueous solution, the mass ratio of water to the ingredients being 1.2, and then the aqueous solution is evaporated at 100° C. to obtain a solid crystal; (3) the solid crystal is crushed into a powder with a particle size of less than 2 mm, and the powder is dried and dehydrated at 160° C. for 4 hours to obtain the powder refining agent.

[0060] Example 5

[0061] The composition and preparation method of the casting aluminum alloy refining and modifying agent in this embodiment are the same as those in Example 1, except that the powder refining agent used in step five is an existing conventional powder refining agent, which is composed of the following components in mass percentage: NaCl 36.13%, KCl 15.42%, CaF2 16.84%, NaF19.24%, and C2Cl6 12.37%. The powder refining agent is obtained by directly crushing and mixing the raw materials after drying and dehydration. In step six, no mixed gas is used, but argon gas with a purity of 99.99% is used to spray, refine, remove slag and degas the aluminum alloy liquid.

[0062] Example 6

[0063] This embodiment uses the refining modifier prepared in Example 1 to refine and modify the cast aluminum alloy to test the effect of the refining and modification. The cast aluminum alloy consists of the following components in mass percentage: Si 17.52%, Cu 4.76%, Mg1.68%, Zn 0.84%, Mn 0.69%, Ni 0.46%, Fe 0.16%, and the balance is Al and unavoidable impurities. The refining and modification method is as follows: the cast aluminum alloy is heated at 700°C to melt into aluminum alloy liquid, and then 0.2% of the weight of the aluminum alloy liquid is added to the refining modifier described in Example 1, and after stirring and melting evenly, the aluminum alloy liquid is cast into a cast aluminum alloy ingot at 690°C.

[0064] Example 7

[0065] This embodiment uses existing conventional Al-5Ti-1B alloy refiner and Al-5Sr alloy modifier for refinement and modification. The composition of the cast aluminum alloy is the same as that of Example 6. The refinement and modification method is as follows: the cast aluminum alloy is heated at 700°C to melt into aluminum alloy liquid, and then 0.2% of the weight of the aluminum alloy liquid by weight of the Al-5Ti-1B alloy refiner and 0.2% of the weight of the aluminum alloy liquid by weight of the Al-5Sr alloy modifier are added. After stirring and melting evenly, the aluminum alloy liquid is cast at 690°C into a cast aluminum alloy ingot.

[0066] Example 8

[0067] In this embodiment, the refining and modifying agent prepared in Example 5 is used to refine and modify the cast aluminum alloy. The composition of the cast aluminum alloy and the refining and modifying method are the same as those in Example 6.

[0068] Verification Example

[0069] The hydrogen content and slag content of the aluminum alloy liquid before casting of Example 1 and Example 5 were tested on site using a hydrogen meter and a slag meter. The results are shown in Table 1. As can be seen from Table 1, the hydrogen content of the aluminum alloy liquid before casting of Example 1 is 0.127 ml / 100 gAl, and the slag content is 0.072 mm 2 / kgAl. Example 5 The hydrogen content of the aluminum alloy liquid before casting is 0.193ml / 100gAl, and the slag content is 0.118mm 2 / kgAl. By comparison, it can be seen that the technical solution of the present invention can obtain a casting aluminum alloy refinement modifier with higher cleanliness.

[0070] Table 1 Hydrogen content and slag content of cast aluminum alloy liquid

[0071]

[0072] Samples were taken from the cast aluminum alloy ingots obtained in Examples 6-8, and after being processed into standard tensile specimens, the room temperature tensile mechanical properties of the specimens were tested on an electronic tensile testing machine, and the results are shown in Table 2. As can be seen from Table 2, the tensile strength of the cast aluminum alloy specimen in Example 6 is 426.1MPa, the yield strength is 371.8MPa, and the elongation after fracture is 10.5%. The tensile strength of the cast aluminum alloy specimen in Example 7 is 365.8MPa, the yield strength is 313.6MPa, and the elongation after fracture is 6.8%. The tensile strength of the cast aluminum alloy specimen in Example 8 is 381.5MPa, the yield strength is 334.5MPa, and the elongation after fracture is 7.2%. By comparison, it can be seen that the strength and plasticity of the cast aluminum alloy in Example 6 are significantly higher than the strength and plasticity of the cast aluminum alloys in Examples 7 and 8.

[0073] Table 2 Tensile mechanical properties of cast aluminum alloy

[0074]

[0075]

[0076] Samples were taken from the cast aluminum alloy ingots before and after refinement and modification in Example 6. After the samples were ground, polished and corroded, the structures of the samples were observed under a microscope. Figure 1 In order to refine the microstructure of the cast aluminum alloy ingot after modification, Figure 2 To refine the microstructure of cast aluminum alloy ingot before modification. Figure 1 It can be seen that after the refinement and modification by the refinement and modification agent of the present invention, the grain structure of the cast aluminum alloy ingot is fine and uniform, and there are no coarse dendritic α-Al grains and coarse needle-shaped or flaky Si phases and Fe-rich phases. Figure 2 It can be seen that the α-Al grains in the microstructure of the cast aluminum alloy ingot are coarse dendrites, and the Si phase and the Fe-rich phase are coarse needle-like. By comparison, it can be seen that the use of the refinement modifier of the present invention can significantly refine and modify the grain structure of the cast aluminum alloy ingot, so that the α-Al grains are transformed from coarse dendrites to fine and uniform ellipsoids or nearly spherical shapes, and the Si phase and the Fe-rich phase are transformed from coarse needle-like shapes to fine fibers or particles.

Claims

1. A casting aluminum alloy refinement modifier, It is characterized in that The refinement modifier is composed of the following components in percentage by mass: Composition: Ti 4.8-5.2%, B 2.4-2.8%, Sr 0.5-1.5%, P 0.05-0.15%, Fe≤0.15%, the balance is Al and other unavoidable impurity elements, the content of each impurity element is ≤0.05%, and the total amount of other impurity elements is ≤0.15%.

2. The casting aluminum alloy refining and modifying agent according to claim 1, It is characterized in that The mass percentages of the B element and the Ti element satisfy: B>Ti×0.45+0.

2.

3. A method for preparing a casting aluminum alloy refining and modifying agent, used for preparing the casting aluminum alloy refining and modifying agent as claimed in claim 1 or 2, It is characterized in that The following steps are included in sequence: Step 1: According to the composition and mass percentage of the refined modifier, aluminum ingot, strontium ingot, aluminum-phosphorus alloy, potassium fluorotitanate and potassium fluoroborate are selected as raw materials for batching; Step 2: Heat the aluminum ingot and melt it into aluminum liquid; Step 3: adding potassium fluorotitanate and potassium fluoroborate to the aluminum liquid, stirring and reacting to obtain aluminum alloy liquid; Step 4: adding strontium ingot and aluminum-phosphorus alloy into aluminum alloy liquid, stirring and melting into aluminum alloy liquid; Step 5: using argon gas and powder refining agent to spray, refine, remove slag and degas the aluminum alloy liquid; Step 6: Use mixed gas to spray, refine, remove slag and degas the aluminum alloy liquid; Step seven: Casting the aluminum alloy liquid into an aluminum alloy ingot to obtain the cast aluminum alloy refining modifier.

4. The method for preparing the casting aluminum alloy refining and modifying agent according to claim 3, It is characterized in that In step 1, the aluminum content of the aluminum ingot is ≥99.7%, the strontium content of the strontium ingot is ≥99.9%, the phosphorus content of the aluminum-phosphorus alloy is 5%, the purity of potassium fluorotitanate is ≥99.5%, and the purity of potassium fluoroborate is ≥99.5%.

5. The method for preparing the casting aluminum alloy refining and modifying agent according to claim 3, It is characterized in that The heating and melting temperature of the aluminum ingot in step 2 is 740-760°C.

6. The method for preparing the casting aluminum alloy refining and modifying agent according to claim 3, It is characterized in that The stirring reaction time in step 3 is 30-60 minutes.

7. The method for preparing the casting aluminum alloy refining and modifying agent according to claim 3, It is characterized in that The purity of the argon gas in step 5 is ≥99.99%, the amount of the powder refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, the temperature of the aluminum alloy liquid during spray refining is 700-720°C, and the spray refining time is 10-20 minutes.

8. The method for preparing the casting aluminum alloy refining and modifying agent according to claim 3, It is characterized in that The powder refining agent in step 5 is composed of the following components in mass percentage: NaCl 35.12%, NaF 19.84%, TiCl 3 16.51%, SrSO 4 10.06%, KPO 3 11.45%, Na 2 B 4 O 7 7.02%, the preparation method of the powder refining agent comprises the following steps in sequence: (1) according to the composition and mass percentage of the powder refining agent, NaCl, NaF, TiCl with a purity of ≥99.8% are selected; 3 、SrSO 4 , KPO 3 、Na 2 B 4 O 7 The steps of: (1) preparing ingredients for the raw materials; (2) adding the ingredients into water at a temperature of 70° C. and stirring to dissolve the ingredients into an aqueous solution, wherein the mass ratio of water to the ingredients is 1.2, and then heating the aqueous solution to 100° C. to evaporate the aqueous solution to obtain solid crystals; and (3) crushing the solid crystals into powders with a particle size of less than 2 mm, and drying and dehydrating the powders at 160° C. for 4 hours to obtain the powder refining agent.

9. The method for preparing the casting aluminum alloy refining and modifying agent according to claim 3, It is characterized in that The mixed gas in step 6 is composed of argon gas with a purity of ≥99.99%, sulfur hexafluoride and carbon monoxide. The volume percentage of sulfur hexafluoride in the mixed gas is 9-11%, the volume percentage of carbon monoxide is 3-5%, the amount of the mixed gas is 2-3 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.3-0.5×10 5 Pa, the temperature of the aluminum alloy liquid during spray refining is 700-720℃, and the spray refining time is 10-15 minutes.

10. The method for preparing the casting aluminum alloy refining and modifying agent according to claim 3, It is characterized in that When the aluminum alloy liquid is cast into an aluminum alloy ingot in step seven, the pouring temperature of the aluminum alloy liquid is 680-700°C.

Citation Information

Patent Citations

  • Grain refinement and modification master alloy for aluminum and aluminum alloy and method for preparing same

    CN101591746A

  • 4032 alloy alterant and use method thereof

    CN101838759A

  • Strontium salt modifier

    CN102127651A

  • Silicon aluminum alloy refining modificator, preparation method of silicon aluminum alloy refining modificator, preparation method of die-casting silicon aluminum alloy and prepared die-casting silicon aluminum alloy

    CN106811614A

  • Rare earth aluminum-titanium-boron grain refiner and preparation method thereof

    CN112011704A