Aluminum-based composite material and preparation method thereof

By using the synergistic effect of nanoTi particles and graphene nanosheets in aluminum-based composite materials, combined with ultrasonic and ball milling technology, the problems of high cost and poor wettability of graphene are solved, and an aluminum-based composite with excellent performance and low cost are prepared. Materials, realize efficient production of materials.

CN119061283AInactive Publication Date: 2024-12-03KUNMING UNIVERSITY

Patent Information

Application Number
CN202411472692.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Due to the high cost and poor wettability of graphene, existing aluminum-based composite materials are difficult to effectively reduce the cost of reinforcement phase and improve the overall performance of the material.

Method used

NanoTi particles, graphene nanosheets and aluminum matrix powder are dispersed in acetone solution, vacuum drying and ball milling after ultrasonic and mechanical stirring, and then pressure sintered under vacuum or high-purity argon, to produce low cost and performance Excellent aluminum-based composite material.

Benefits of technology

By breaking up the enhanced phase particles, wettability of graphene and metal matrix is ​​improved, slag inclusions and pores are reduced, the comprehensive performance of the material is improved, production costs are reduced, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061283A_ABST
    Figure CN119061283A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of materials. The invention provides an aluminum-based composite material and a preparation method thereof.The method comprises the steps that nano Ti particles, graphene nanosheets and aluminum matrix powder are dispersed in an acetone solution, and mixed slurry is obtained; performing vacuum drying on the obtained mixed slurry to obtain solid composite powder; the solid composite powder is subjected to ball milling, and aluminum-based composite particles obtained after ball milling are obtained; and under vacuum or high-purity argon, the ball-milled aluminum-based composite particles are subjected to pressure sintering, and finally the aluminum-based composite material is prepared. According to the invention, nano Ti particles and graphene are used as a reinforcement phase, so that the cost of the reinforcement phase is reduced, metal Ti particles also effectively improve the wettability of graphene and a metal matrix, agglomeration among the particles is scattered by an ultrasonic combined ball milling process, crystal grains are refined, slag inclusion and pores of the composite material are reduced, and the composite material has good mechanical properties. And the comprehensive performance of the aluminum-based composite material is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of materials, and in particular to an aluminum-based composite material and a preparation method thereof. Background Art

[0002] With the continuous development of the nuclear industry, new energy vehicle field, aerospace, etc., higher requirements are also put forward for the high performance and lightweight of metal materials. Lightweight aluminum alloys are used in the fields of automobiles, aerospace, electronic mobile devices, etc. due to their good mechanical properties, excellent heat resistance, electrical conductivity, corrosion resistance and lightness. Aluminum-based composite materials made by adding reinforcing materials have better comprehensive performance than the matrix. One of the reinforcing materials is graphene, which was obtained by the GEIM team in 2004 by separating graphite. It is a two-dimensional crystalline material formed by a single layer of closely arranged carbon atoms. It is the thinnest and strongest material discovered so far. The addition of graphene can improve the performance of the aluminum matrix. However, since graphene is expensive, easy to agglomerate, and has poor wettability with the matrix, it is necessary to provide a method for preparing aluminum-based composite materials that reduces the cost of the reinforcing phase and improves the wettability of graphene. Summary of the invention

[0003] The purpose of the present invention is to solve the defects of the above-mentioned prior art and provide an aluminum-based composite material with low cost and excellent reinforcement phase and a preparation method thereof.

[0004] A method for preparing an aluminum-based composite material comprises the following steps: Step 1: dispersing nano-Ti particles, graphene nanosheets and aluminum matrix powder in an acetone solution to obtain a mixed slurry; Step 2: vacuum drying the obtained mixed slurry to obtain a solid composite powder; Step 3: ball-milling the solid composite powder to obtain ball-milled aluminum-based composite particles; Step 4: Under vacuum or high-purity argon, the ball-milled aluminum-based composite particles are pressure-sintered to finally prepare an aluminum-based composite material.

[0005] Furthermore, in the method for preparing the aluminum-based composite material as described above, step 1 comprises: The nano-Ti particles, graphene nanosheets and aluminum alloy powder are dispersed in acetone by ultrasonication and mechanical stirring respectively; then the mixture of the three is ultrasonicated again and mechanically stirred for 10 minutes to finally obtain the mixed slurry.

[0006] Furthermore, in the method for preparing the aluminum-based composite material as described above, step 2 comprises: The mixed slurry was heated at 65 The solid composite powder was finally obtained by vacuum drying for 24 hours.

[0007] Furthermore, in the method for preparing the aluminum-based composite material as described above, step 3 comprises: The solid composite powder is placed in a stainless steel vacuum ball mill, an agate ball with a diameter of 10 is selected for loading, and then vacuum is drawn. The ball milling time is 3 hours, the rotation speed is 200r / min, and the ball milling is paused for 30 minutes and cooled for 10 minutes to obtain the aluminum-based composite particles.

[0008] Furthermore, in the above-mentioned method for preparing the aluminum-based composite material, the mass ratio of the agate balls to the solid composite powder is 10:1.

[0009] Furthermore, in the method for preparing the aluminum-based composite material as described above, step 4 comprises: The composite particles obtained after ball milling are placed in a hot pressing sintering furnace for pressure sintering; The pressure sintering is performed under vacuum or high-purity argon protection.

[0010] Further, in the above-mentioned method for preparing the aluminum-based composite material, in step 4, the pressure sintering conditions are: Sintering temperature: 540℃, heating rate: 5℃ / min, holding time: 120min, axial pressure 30Mpa.

[0011] Furthermore, in the method for preparing the aluminum-based composite material as described above, the nano-Ti particles, graphene nanosheets and aluminum matrix powder, measured by mass percentage, include: Graphene nanosheets: 0.1-0.9wt%; Ti particles: 0.3-5wt%; Balance: aluminum matrix powder.

[0012] The aluminum-based composite material is prepared by any of the above methods.

[0013] The method provided by the present invention reduces the cost of the reinforcement phase by using Ti and graphene as the reinforcement phase; at the same time, the metal Ti particles effectively improve the wettability of the graphene and the metal matrix. The present invention breaks up the agglomeration of the reinforcement phase particles by pressure sintering the aluminum-based composite particles after ultrasound and ball milling; and enhances the nano-Ti particles, effectively improving the wettability of the graphene nanosheets and the metal matrix, making them well combined, improving the agglomeration tendency of the particles, refining the grains, reducing the slag inclusions and pores of the composite material, and effectively improving the comprehensive performance of the aluminum-based composite material.

[0014] The present invention ball-mills solid composite powder and pressure-sinters the milled aluminum-based composite particles, thereby being able to manufacture parts with complex shapes and structures, reducing material waste, having a low sintering temperature, and relatively simplifying the production process. It does not require complex processing steps and expensive mechanical equipment, further reducing production costs, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a schematic diagram of the cross section of the tensile specimen; Figure 2 (a) is a dimensional diagram of the tensile specimen in the front view; FIG2( b ) is a right side view of FIG2( a ); Figure 2 (c) is a top view; Figure 3 This is the fracture morphology of Example 2; Figure 4 This is the fracture morphology of Example 3. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0017] This embodiment provides a method for preparing an aluminum-based composite material, and the specific preparation steps are as follows: Step 1: Place nano-Ti particles (0.3wt%), graphene nanosheets (0.3wt%) and aluminum alloy powder in acetone, perform ultrasonic and mechanical stirring for 10 min, mix the three, and perform ultrasonic and mechanical stirring for 10 min again. The ultrasonic treatment frequency is 20kHz and the power is 2000w to obtain a uniformly dispersed mixed slurry. The mixture was dried under vacuum for 24 h to obtain a solid composite powder.

[0018] Step 2: Place the solid composite powder obtained above in a stainless steel vacuum ball mill for ball milling, further disperse the reinforcement phase evenly in the matrix, select agate balls with a diameter of 10 mm, and load them with a ball-to-material ratio of 10:1, and then evacuate. Intermittent ball milling is used, with a total ball milling time of 3 hours. After 30 minutes of ball milling, pause and cool for 10 minutes to avoid excessive heat generated during the ball milling process and affect the ball milling efficiency. The ball mill speed is set to 200r / min, and low-speed mixing is performed to reduce damage to the graphene structure. After the ball milling, reinforced aluminum-based composite particles are obtained.

[0019] The present invention performs ultrasonic and mechanical stirring treatments on nano-Ti particles, graphene nano-sheets and aluminum alloy powder twice in succession, so that the nano-Ti particles and graphene nano-sheets can be mixed more evenly and thus can be more evenly dispersed in the aluminum matrix.

[0020] Step 3: Under the protection of high-purity argon, the aluminum-based composite particles obtained by ball milling are placed in a pressure sintering furnace for sintering at a sintering temperature of 540°C, a heating rate of 5°C / min, a holding time of 120min, and an axial pressure of 30Mpa to obtain a Ti-hybrid graphene-reinforced aluminum-based composite material. Example

[0021] This embodiment provides a method for preparing a Ti-hybrid graphene reinforced aluminum-based composite material, and the specific preparation steps are as follows: Step 1: Place nano-Ti particles (0.9wt%), graphene nanosheets (0.3wt%) and aluminum alloy powder in acetone, perform ultrasonic and mechanical stirring for 10 min, and then mix the three and perform ultrasonic and mechanical stirring for 10 min. The ultrasonic treatment frequency is 20kHz and the power is 2000w to obtain a uniformly dispersed mixed slurry. The mixture was dried under vacuum for 24 h to obtain a solid composite powder.

[0022] Step 2: Place the solid composite powder obtained above in a stainless steel vacuum ball mill for ball milling, further disperse the reinforcement phase evenly in the matrix, select agate balls with a diameter of 10 mm, and load them with a ball-to-material ratio of 10:1, and then evacuate. Intermittent ball milling is used, with a total ball milling time of 3 hours. After 30 minutes of ball milling, pause and cool for 10 minutes to avoid excessive heat generated during the ball milling process and affect the ball milling efficiency. The ball mill speed is set to 200r / min, and low-speed mixing is performed to reduce damage to the graphene structure. After the ball milling, reinforced aluminum-based composite particles are obtained.

[0023] Step 3: Under the protection of high-purity argon, the aluminum-based composite particles obtained by ball milling are placed in a pressure sintering furnace for sintering at a sintering temperature of 540°C, a heating rate of 5°C / min, a holding time of 120min, and an axial pressure of 30Mpa to obtain a Ti-hybrid graphene-reinforced aluminum-based composite material. Example

[0024] This embodiment provides a method for preparing a Ti-hybrid graphene reinforced aluminum-based composite material, and the specific preparation steps are as follows: Step 1: Place nano-Ti particles (1.5wt%), graphene nanosheets (0.3wt%) and aluminum alloy powder in acetone, perform ultrasonic and mechanical stirring for 10 min, and then mix the three and perform ultrasonic and mechanical stirring for 10 min. The ultrasonic treatment frequency is 20kHz and the power is 2000w to obtain a uniformly dispersed mixed slurry. The mixture was dried under vacuum for 24 h to obtain a solid composite powder.

[0025] Step 2: Place the solid composite powder obtained above in a stainless steel vacuum ball mill for ball milling, further disperse the reinforcement phase evenly in the matrix, select agate balls with a diameter of 10 mm, and load them with a ball-to-material ratio of 10:1, and then evacuate. Intermittent ball milling is used, with a total ball milling time of 3 hours. After 30 minutes of ball milling, pause and cool for 10 minutes to avoid excessive heat generated during the ball milling process and affect the ball milling efficiency. The ball mill speed is set to 200r / min, and low-speed mixing is performed to reduce damage to the graphene structure. After the ball milling, reinforced aluminum-based composite particles are obtained.

[0026] Step 3: Under the protection of high-purity argon, the aluminum-based composite particles obtained by ball milling are placed in a pressure sintering furnace for sintering at a sintering temperature of 540°C, a heating rate of 5°C / min, a holding time of 120min, and an axial pressure of 30Mpa to obtain a Ti-hybrid graphene-reinforced aluminum-based composite material.

[0027] Comparative Example 1: Step 1: Place aluminum alloy powder (100 wt%) in acetone and perform ultrasonic treatment accompanied by mechanical stirring for 10 min. The ultrasonic treatment frequency is 20 kHz and the power is 2000 W to obtain a liquid dispersion slurry. Dry under vacuum for 24 h to obtain a solid powder.

[0028] Step 2: Place the solid powder obtained above in a stainless steel vacuum ball mill for ball milling. Select agate balls with a diameter of 10 mm and a ball-to-material ratio of 10:1 for loading, and then evacuate. Use intermittent ball milling, with a total ball milling time of 3 hours. After 30 minutes of ball milling, pause and cool for 10 minutes to avoid excessive heat generation during the ball milling process that affects the ball milling efficiency. The ball mill speed is set to 200r / min, and solid powder is obtained after the ball milling is completed.

[0029] Step 3: Under the protection of high-purity argon, the aluminum-based powder obtained by ball milling is placed in a pressure sintering furnace for sintering at a sintering temperature of 540°C, a heating rate of 5°C / min, a holding time of 120min, and an axial pressure of 30Mpa to obtain an aluminum alloy matrix block.

[0030] Comparative Example 2: Step 1: Place graphene nanosheets (0.3 wt%) and aluminum alloy powder in acetone, perform ultrasonic and mechanical stirring for 10 min, and then mix the two and perform ultrasonic and mechanical stirring for 10 min. The ultrasonic treatment frequency is 20 kHz and the power is 2000 W to obtain a uniformly dispersed mixed slurry. The mixture was dried under vacuum for 24 h to obtain a solid composite powder.

[0031] Step 2: Place the solid composite powder obtained above in a stainless steel vacuum ball mill for ball milling, further disperse the reinforcement phase evenly in the matrix, select agate balls with a diameter of 10 mm, and load them with a ball-to-material ratio of 10:1, and then evacuate. Intermittent ball milling is used, with a total ball milling time of 3 hours. After 30 minutes of ball milling, pause and cool for 10 minutes to avoid excessive heat generated during the ball milling process and affect the ball milling efficiency. The ball mill speed is set to 200r / min, and low-speed mixing is performed to reduce damage to the graphene structure. After the ball milling, reinforced aluminum-based composite particles are obtained.

[0032] Step 3: Under the protection of high-purity argon, the aluminum-based composite particles obtained by ball milling are placed in a pressure sintering furnace for sintering at a sintering temperature of 540°C, a heating rate of 5°C / min, a holding time of 120min, and an axial pressure of 30Mpa to obtain a graphene-reinforced aluminum-based composite material.

[0033] The prepared composite material was made into a tensile test piece. Figure 1 Figure 2 is a schematic diagram of the cross section of the tensile specimen; Figure 2 (a)-(c) is the dimension diagram of the tensile specimen (unit: mm); the tensile equipment is Zwick / Roell Z250, and the tensile rate is 0.5 mm / min. The test performance is shown in Table 1.

[0034] Table 1: Performance table of examples and comparative examples

[0035] Compared with Comparative Example 1-2, Example 1-3 has the same processes except that the raw material ratio is different from that of Comparative Example 1-2. As can be seen from the product performance table 1, the yield strength and tensile strength of Examples 1, 2 and 3 are significantly better than those of Comparative Examples 1 and 2.

[0036] Depend on Figure 3 and Figure 4 From the fracture morphology, it can be seen that the fracture presents a dimple fracture, indicating that the increase of nano-Ti particles enhances the strength of the composite material while maintaining good plasticity.

[0037] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an aluminum-based composite material, characterized in that: The following steps are involved: Step 1: dispersing nano-Ti particles, graphene nanosheets and aluminum matrix powder in an acetone solution to obtain a mixed slurry; Step 2: vacuum drying the obtained mixed slurry to obtain a solid composite powder; Step 3: ball-milling the solid composite powder to obtain ball-milled aluminum-based composite particles; Step 4: Under vacuum or high-purity argon, the ball-milled aluminum-based composite particles are pressure-sintered to finally prepare an aluminum-based composite material.

2. The method for preparing the aluminum-based composite material according to claim 1, characterized in that: The step 1 comprises: The nano-Ti particles, graphene nanosheets and aluminum alloy powder are dispersed in acetone by ultrasonication and mechanical stirring; then the mixture of the three is ultrasonicated again and mechanically stirred for 10 minutes to finally obtain the mixed slurry.

3. The method for preparing the aluminum-based composite material according to claim 1, characterized in that: The step 2 comprises: The mixed slurry was vacuum dried at 65° C. for 24 h to finally obtain the solid composite powder.

4. The method for preparing the aluminum-based composite material according to claim 1, characterized in that: The step 3 comprises: The solid composite powder is placed in a stainless steel vacuum ball mill, an agate ball with a diameter of 10 mm is selected for loading, and then vacuum is drawn. The ball milling time is 3 hours, the rotation speed is 200 r / min, and an intermittent ball milling method is adopted. After ball milling for 30 minutes, the cooling is paused for 10 minutes to obtain the aluminum-based composite particles.

5. The method for preparing the aluminum-based composite material according to claim 4, characterized in that: The mass ratio of the agate balls to the solid composite powder is 10:

1.

6. The method for preparing the aluminum-based composite material according to claim 1, characterized in that: The step 4 comprises: The composite particles obtained after ball milling are placed in a hot pressing sintering furnace for pressure sintering; The pressure sintering is performed under vacuum or high-purity argon protection.

7. The method for preparing the aluminum-based composite material according to claim 6, characterized in that: In step 4, the conditions for pressure sintering are: Sintering temperature: 540℃, heating rate: 5℃ / min, holding time: 120min, axial pressure 30Mpa.

8. The method for preparing the aluminum-based composite material according to claim 1, characterized in that: The nano-Ti particles, graphene nano-sheets and aluminum matrix powder include, by mass percentage: Graphene nanosheets: 0.1-0.9wt%; Ti particles: 0.3-5wt%; Balance: aluminum matrix powder.

9. An aluminum-based composite material prepared by the method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Graphene-containing titanium-aluminum-base self-lubricating composite material and preparation method thereof

    CN103334030A

  • Method for preparing graphene reinforced aluminum matrix composite material by microwave sintering

    CN105861865A

  • Preparing method for cast graphene / aluminum alloy composite material and cast graphene / aluminum alloy composite material

    CN107502772A

  • Preparation method of silicone oil repair graphene reinforced aluminum base composite material

    CN109128134A

  • Carbon nano-tube and endogenetic nanometer TiC particle hybrid reinforced aluminum matrix composite and preparation method thereof

    CN109652679A