AlFeNiTiV high-entropy alloy material and preparation method thereof
By adjusting the composition of AlFeNiTiV high-entropy alloy and vacuum argon arc smelting method, the BCC and L21 phase structure are optimized, and the problem of insufficient high-temperature performance of lightweight high-entropy alloys is solved, and the combination of low density, high strength and excellent high-temperature mechanical properties is achieved. , suitable for aerospace and energy transportation fields.
Patent Information
- Application Number
- CN202411121429.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing lightweight high-entropy alloys have insufficient research on high-temperature performance, the performance limits of traditional alloys are difficult to break through, and the mechanical performance regulation rules are unclear, which limits their application, especially in the fields of aerospace and energy transportation, which cannot meet the needs.
By adjusting the composition of AlFeNiTiV high-entropy alloy, the synergistic enhancement effect of the BCC-(Fe,V) phase and L21-(Ni2AlTi) phase is optimized, and the alloy is prepared by vacuum argon arc smelting method to form a biphasic structure of BCC+L21 to achieve low Combination of density, high strength and excellent high temperature yield strength.
The combination of low density, high strength and excellent high temperature mechanical properties is achieved, and the mechanical properties of the alloy is improved, showing room temperature yield strength of 2140MPa and specific yield strength of 314.4MPa·cm3/g, and maintaining high compression yield at 600-700℃. Strength and plasticity, suitable for different application environments.
Smart Images

Figure CN119061305A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of materials, and in particular to an AlFeNiTiV high entropy alloy material and a preparation method thereof. Background Art
[0002] At present, the operating temperature of traditional nickel-based superalloys widely used in gas turbines and aircraft engines has reached 80% of their melting point, which cannot meet the more stringent operating conditions brought about by further increases in operating temperature. In addition, nickel-based superalloys also have the disadvantages of being expensive and high-density, so there is an urgent need to develop a new generation of lightweight, high-strength, low-cost high-temperature application structural alloys.
[0003] Among the reported lightweight high-entropy alloys, according to the characteristics of the elements, the systems can be roughly divided into three categories: alloy systems based on conventional metal elements Al, Co, Cr, Fe, and Ni, alloy systems containing one or several refractory metal elements Nb, W, Mo, and Ta, and alloy systems containing ultra-low density elements such as Mg and Li. Among them, the density of most high-entropy alloy systems based on Al, Mg, Li, Zn, and Ti is ≤4.5g / cm 3 (traditional titanium alloy), with a hardness of ≥400HV, is a lightweight high-entropy alloy system with a relatively high specific hardness, and has been widely studied by many scholars. However, the specific yield strength of the lightweight high-entropy alloys currently prepared is generally small, which cannot further meet the needs of some aerospace, energy and transportation fields that require lightweight and high-strength materials.
[0004] The presence of ordered phases or intermetallic phases makes high-entropy alloys exhibit high strength. In recent years, many studies have shown that the Ni2AlTi structure with Huesler structure, as an ordered variant of the B2 structure, has become a prominent research focus due to its good properties, such as cost-effectiveness, low density, and excellent high-temperature creep resistance. However, although the limited slip system of the L21 phase can enhance the performance of the alloy, it will make the alloy brittle at room temperature. Recently, some research reports pointed out that the L21+BCC dual-phase structure has similar crystal structure and low lattice mismatch, and has attracted much attention due to its excellent ductility and high-temperature performance. This not only maintains the high thermal stability of the L21 phase, but also exhibits excellent strength at both room temperature and high temperature. However, due to the unclear regulation of its mechanical properties, there is no regularity to improve the mechanical properties of the alloy, lacks a systematic guidance method, and cannot flexibly adapt to the needs of different application environments.
[0005] In general, the development of lightweight, high-strength, high-entropy alloys has made significant progress, but there are still defects and shortcomings: (1) There is still very little research on the high-temperature performance of lightweight high-entropy alloys, which needs further research and improvement. Judging from the current development trend of lightweight high-strength alloys, it is difficult to achieve a major breakthrough in the performance limit of traditional lightweight alloys. (2) Most lightweight high-entropy alloys have BCC phase and multiphase structures and are brittle at room temperature. However, due to the unclear regulation rules of their mechanical properties and the lack of systematic guidance methods, their further application is limited. Summary of the invention
[0006] In view of the above technical problems, the present invention discloses an AlFeNiTiV high entropy alloy material and a preparation method thereof. By adjusting appropriate components, the synergistic reinforcement effect of the BCC-(Fe, V) phase and the L21-(Ni2AlTi) phase in the alloy is improved, the performance of the L21 strengthened alloy is optimized, and the alloy exhibits a combination of low density, high strength and excellent high temperature specific yield strength, which has broad application prospects.
[0007] To this end, the technical solution adopted by the present invention is:
[0008] An AlFeNiTiV high entropy alloy material, the composition of which is Al 15 Fe x Ni 30 Ti 15 V 40-x , where 30≤x≤40.
[0009] By adopting this technical solution and selecting appropriate components, the alloy material can improve the synergistic reinforcement effect of the BCC-(Fe, V) phase and the L21-(Ni2AlTi) phase in the alloy, optimize the performance of the L21 strengthened alloy, and make it exhibit a combination of low density, high strength, and excellent high-temperature specific yield strength, which has broad application prospects.
[0010] As a further improvement of the present invention, x=35 or 40.
[0011] The present invention also discloses a method for preparing the AlFeNiTiV high entropy alloy material as described above, comprising the following steps:
[0012] Step S1, according to Al 15 Fe x Ni 30 Ti 15 V 40-x According to the nominal ratio, Al, Fe, Ni, Ti and V particles are weighed and alloy ingots are prepared by vacuum argon arc melting method;
[0013] Step S2, when the vacuum degree reaches 5×10 -3When the vacuum degree is below Pa, protective argon gas is introduced to a vacuum degree of -0.025 Pa, and the alloy ingot is remelted multiple times.
[0014] By adopting this technical solution, the preparation method is simple, and the synergistic reinforcement effect of the BCC-(Fe, V) phase and the L21-(Ni2AlTi) phase in the alloy can be improved by adjusting the appropriate composition.
[0015] As a further improvement of the present invention, in step S2, remelting is performed 5 times, and each melting time is 3 minutes.
[0016] As a further improvement of the present invention, the welding machine current in the vacuum argon arc melting method is 230A.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The technical solution of the present invention is used to design the composition of the light alloy in combination with the concept of high entropy alloy. 15 Fe x Ni 30 Ti 15 V 40-x Lightweight high entropy alloys remove the expensive element Co to reduce costs based on conventional light alloy systems. By properly adjusting the composition of the BCC-(Fe, V) phase in the alloy, it has a synergistic strengthening effect of multiple strengthening methods such as solid solution strengthening, grain boundary strengthening, and second phase strengthening. While sacrificing a relatively small density, it greatly improves the mechanical properties of the alloy, showing excellent properties of low density, high strength, and excellent high temperature specific yield strength. The technical solution of the present invention is Al 15 Fe 35 Ni 30 Ti 15 V5 high entropy alloy has a dual-phase structure of BCC+L21, and the interface between the two phases is a semi-coherent interface, which reduces the dislocation migration rate during deformation and ultimately achieves a significant increase in yield strength while maintaining a low density of 6.81g / cm 3 Under the premise of room temperature yield strength of 2140MPa and specific yield strength of 314.4MPa·cm 3 / g excellent technical indicators. In addition, Al 15 Fe 35 Ni 30 Ti 15 The V5 composition high-entropy alloy also exhibits excellent high-temperature mechanical properties, showing high compressive yield strength (1612MPa and 972MPa) and high compressive plasticity (25% and 33%) at 600 and 700°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is Al of different x in the embodiment of the present invention15 Fe x Ni 30 Ti 15 V 40-x SEM micrographs of high entropy alloys; where (a) x=0, (b) x=10, (c) x=20, (d) x=30, (e) x=35, and (f) x=40.
[0020] Figure 2 is Al of different x in the embodiment of the present invention 15 Fe x Ni 30 Ti 15 V 40-x The phase of the alloy, where (a) is Al 15 Fe x Ni 30 Ti 15 V 40-x Figure 2 XRD patterns of the alloys with x=0, 10, 20, 30, 35 and 40%, (b) is an enlarged view of the 2θ angle range between 42 and 46 degrees in (a), and (c) is a fitting diagram of the (110) BCC and (220) L21 peaks of the alloys with x=10 and x=30 using the pseudo-Voigt function.
[0021] Figure 3 is Al of different x in the embodiment of the present invention 15 Fe x Ni 30 Ti 15 V 40-x IPF diagram of high entropy alloy, where (a) x=0, (b) x=10, (c) x=20, (d) x=30, (e) x=35, (f) x=40.
[0022] Figure 4 is Al of different x in the embodiment of the present invention 15 Fe x Ni 30 Ti 15 V 40-x Density comparison chart of high entropy alloys.
[0023] Figure 5 is Al of different x in the embodiment of the present invention 15 Fe x Ni 30 Ti 15 V 40-x Hardness comparison chart of high entropy alloys.
[0024] Figure 6 is Al of different x in the embodiment of the present invention 15 Fe x Ni30 Ti 15 V 40-x Compressive stress-strain curves of high entropy alloys.
[0025] Figure 7 is Al of different x in the embodiment of the present invention 15 Fe x Ni 30 Ti 15 V 40-x Fracture morphology of high entropy alloy; where (a) x=0, (b) x=20, (c) x=35, (d) x=40.
[0026] Figure 8 is Al of the embodiment of the present invention 15 Fe 35 Ni 30 Ti 15 High temperature compressive stress-strain curves of V5 high entropy alloy at 600-900℃.
[0027] Fig. 9 is Al of the embodiment of the present invention 15 Fe 35 Ni 30 Ti 15 IPF and grain boundary diagrams of V5 high entropy alloy deformed at high temperatures, where (a) and (a1) are the IPF and grain boundary diagrams at 600°C, and (b) and (b1) are the IPF and grain boundary diagrams at 800°C.
[0028] Fig.10 is Al of the embodiment of the present invention 15 Fe x Ni 30 Ti 15 V 40-x Vertical cross-section of the CCAs phase diagram for different x values of the alloy. DETAILED DESCRIPTION
[0029] The preferred embodiments of the present invention are described in further detail below.
[0030] An AlFeNiTiV high entropy alloy material, the composition of which is Al 15 Fe x Ni 30 Ti 15 V 40-x (hereinafter referred to as AlFeNiTiV), wherein 30≤x≤40. The preparation method comprises:
[0031] According to the nominal ratio, the raw materials are Al, Fe, Ni, Ti, and V particles with a purity of 99.99wt.%, and the alloy ingots with the designed composition are prepared by vacuum argon arc melting.-3 When the pressure was below Pa, protective argon gas was introduced until the vacuum degree was -0.025Pa. To ensure chemical uniformity, the alloy was remelted 5 times, each melting time was 3 minutes, and the welding current was 230A.
[0032] According to the above method, alloys with different x are prepared, and x=0, 10, 20, 30, 35, 40, that is, x represents the at.% content of Fe.
[0033] Under different Fe contents, Al 15 Fe x Ni 30 Ti 15 V 40-x The SEM morphology of the alloy material is as follows Figure 1 As shown in the SEM morphology, it can be seen that the addition of Fe causes the microstructure of the alloy to change from a dendrite structure to a mesh structure. The alloy material presents two phases with different contrasts in the backscattering mode, namely a dark phase (rich in Al, Ni, Ti) and a bright phase (rich in Fe, V). When the Fe content is below 30 at.%, in addition to the above two phases, a bright white phase is found at the interface between the two phases, which is the intermetallic compound Laves phase. The presence of the Laves brittle phase will cause the interface to become a crack source, and the mechanical properties of the alloy will decrease. Figure 2 The XRD patterns of high entropy alloys with different Fe contents are shown in Table 1. The alloys are mainly composed of disordered BCC and ordered L21 phases, corresponding to Figure 1 The bright phase (rich in Fe, V) and dark phase (rich in Al, Ni, Ti) of the BCC phase are shown in Figure 2. As the Fe content continues to increase, the BCC phase diffraction peak shifts to the right, the lattice constant of the BCC phase continues to decrease, and a brittle phase exists when the Fe addition amount is 0at.% and 10at.%, corresponding to Figure 1 The bright white phase (Fe- and Ti-rich Laves phase) in the alloy was not observed in the XRD of the alloys with Fe addition of 20 at.% and 30 at.% due to the low content. Figure 3 For Al 15 Fe x Ni 30 Ti 15 V 40-x From the IPF diagram of the EBSD of the alloy material, it can be observed that with the continuous increase of Fe content, the alloy grains change from columnar dendrites to equiaxed crystals, and the grains of the equiaxed crystals remain basically unchanged after continuous refinement. According to the Hall-Page formula, the continuous increase in the degree of grain refinement makes the number of grain boundaries increase accordingly, and the strength gain effect brought by grain boundary strengthening also increases accordingly. Figure 4 Given Al 15 Fe x Ni 30 Ti 15 V40-x The density of the alloy material changes with the increase of Fe content, indicating that the increase of Fe content will lead to a slight increase in the alloy density, but it is still within the definition of lightweight high entropy alloy (7g / cm 3 ) range. Figure 5 For Al 15 Fe x Ni 30 Ti 15 V 40-x The hardness change diagram of the alloy material shows that the addition of Fe causes the hardness of the alloy to increase first and then decrease, reaching the maximum value when the Fe addition amount is 35at.%. 15 Fe x Ni 30 Ti 15 V 40-x The compressive stress-strain curve of alloy materials is as follows Figure 6 As shown in the figure, it shows that with the continuous increase of Fe content, the gain effect brought by solid solution strengthening and grain boundary strengthening continues to increase, the yield strength of the alloy first increases and then decreases, but the plasticity shows a trend of first significantly decreasing and then increasing. When the Fe addition amount of the alloy is 10at.%, the plasticity of the alloy decreases significantly due to the presence of Laves brittle phase, and the compressive fracture strength also decreases. Figure 7 These are the SEM images of the compression fracture with Fe addition of 0, 20, 35, and 40at.%. It can be seen that when the Fe addition is 0at.%, there are a large number of dimples on the fracture, which is a ductile fracture; when the Fe addition is 20at.%, the alloy fracture presents a river-like and cleavage step morphology, which is a typical brittle fracture feature; when the Fe addition increases to 35at.%, the macroscopic port morphology shows the characteristics of typical intergranular fracture, and the microscopic image of the fracture shows that there are also a small amount of transgranular fracture characteristics; when the Fe addition is 40at.%, cracks can be observed on the fracture, the fracture surface is relatively smooth and there are a small number of dimples, which is a combination of ductile and brittle fracture characteristics.
[0034] The technical solution of the present invention aims to obtain a lightweight high-entropy alloy with excellent mechanical properties and low density. The AlFeNiTiV lightweight high-entropy alloy is prepared and optimized by vacuum argon arc melting. The optimal Fe content is selected according to the mechanical properties of the cast alloy, and Al is selected within the definition range of the lightweight high-entropy alloy density. 15 Fe 35 Ni 30 Ti 15 V5 high entropy alloy is used as the optimal composition.
[0035] The results show that under the synergistic effect of BCC and L21 phases, Al 15 Fe 35 Ni 30 Ti15 The density of V5 high entropy alloy is 6.81g / cm 3 The compressive yield strength and plasticity are 2140MPa and 6.7% respectively, and the specific yield strength is as high as 314.4MPa·cm 3 / g, achieving a combination of low density and excellent mechanical properties. High temperature compression test was carried out on the alloy with this composition. Figure 8 For Al 15 Fe 35 Ni 30 Ti 15 High temperature compression stress-strain curve of V5 high entropy alloy at 600-900℃. When the test temperature is increased from room temperature to 600℃ and 700℃, the strength of the alloy decreases and the deformation capacity increases. The yield strength of the alloy is 1612MPa and 972Mpa respectively, and the compression plasticity reaches 25% and 33%. At 800℃, the yield strength of the alloy is further reduced to 536MPa. At a high temperature of 900℃, the yield strength of the alloy drops sharply to 196MPa, and the strain exceeds 50% during the compression process, and no fracture occurs, indicating that the alloy has excellent high temperature mechanical properties.
[0036] In order to study the microstructural evolution during high temperature softening, Fig. 9 The EBSD images of the central area of the cross section of the Fe35 alloy after compression fracture at two characteristic temperatures (600℃ and 800℃) are shown. Fig. 9 It can be seen that with the increase of deformation temperature, the grain size of the alloy increases slightly. When deformed at 600℃, no recrystallized grains were observed inside the alloy, indicating that dynamic recovery is still the main mechanism inside the alloy. A lower proportion of dynamic recrystallization (DRX) can be observed in the microstructure of the alloy deformed at 800℃, but the high temperature softening mechanism of the alloy is still dominated by dynamic recovery. The presence of DRX reduces the deformation resistance of the metal material and increases its plasticity, resulting in an increase in the ductility of the alloy and a decrease in the yield strength. It is worth noting that from Al2O3 at different temperatures 15 Fe 35 Ni 30 Ti 15 From the stress-strain curve of V5 alloy, the yield strength of the alloy at 900°C is greatly reduced.
[0037] CALPHAD calculations divide the different components of Al 15 Fe x Ni 30 Ti 15 V 40-x The solidification path of the alloy was established. 15 Fe x Ni 30 Ti 15 V 40-xA vertical cross section of the phase diagram is Fig.10 As shown. 15 Fe 35 Ni 30 Ti 15 The V5 alloy undergoes BCC-FCC phase transformation at about 900℃, which may be the reason why the yield strength is greatly reduced at high temperature of 900℃.
[0038] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. An AlFeNiTiV high entropy alloy material, characterized in that: Its composition is Al 15 Fe x Ni 30 Ti 15 V 40-x , where 30≤x≤40.
2. The AlFeNiTiV high entropy alloy material according to claim 1, characterized in that: x=35 or 40.
3. The method for preparing the AlFeNiTiV high entropy alloy material according to claim 1 or 2, characterized in that: The steps include: Step S1, according to Al 15 Fe x Ni 30 Ti 15 V 40-x According to the nominal ratio, Al, Fe, Ni, Ti and V particles are weighed and alloy ingots are prepared by vacuum argon arc melting method; Step S2, when the vacuum degree reaches 5×10 -3 When the vacuum degree is below Pa, protective argon gas is introduced to a vacuum degree of -0.025 Pa, and the alloy ingot is remelted multiple times.
4. The method for preparing the AlFeNiTiV high entropy alloy material according to claim 3, characterized in that: In step S2, remelting is performed 5 times, and each remelting time is 3 minutes.
5. The method for preparing the AlFeNiTiV high entropy alloy material according to claim 3, characterized in that: The welding current in the vacuum argon arc melting method is 230A.
Citation Information
Patent Citations
AlFeCoNiCrTiVx high-entropy alloy material and preparation method thereof
CN103194657A
High-entropy alloy based on solid solution and precipitation strengthening effect and preparation method thereof
CN112813332A
Lightweight high-strength corrosion-resistant high-entropy alloy and preparation method thereof
CN114231818A
AlCrFeNiTi high-entropy alloy material and preparation method thereof
CN116463535A
Soft magnetic high-entropy alloy
RU2824638C1