WNbMoTaTiC series high-temperature high-entropy alloy containing eutectic structure and preparation method thereof
A WNbMoTaTiC-based high-entropy alloy with a eutectic structure addresses the limitations of traditional alloys by enhancing strength, plasticity, and fluidity, offering improved performance and lower density for high-temperature applications.
Patent Information
- Application Number
- CN202411334409.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional refractory high-entropy alloys like WNbMoTa and WNbMoTaV exhibit high strength but low plasticity and poor fluidity, making them difficult to form precision workpieces, and their density is high, which increases costs.
A WNbMoTaTiC-based high-entropy alloy with a eutectic structure is developed, composed of specific atomic percentages of W, Nb, Mo, Ta, and C, prepared using a non-consumable vacuum arc melting furnace with controlled melting and magnetic stirring to ensure uniformity.
The alloy achieves higher room temperature strength and plasticity, lower density, and better fluidity, with room temperature yield strength up to 2590MPa and elongation over 10%, and density less than 15g/cm³, while maintaining high-temperature performance.
Smart Images

Figure CN119061306A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of high-temperature high-entropy alloys, and in particular to a WNbMoTaTiC-based high-temperature high-entropy alloy containing a eutectic structure and a preparation method thereof. Background Art
[0002] High entropy alloys are different from traditional alloys. They have multiple principal elements, and the alloy matrix is usually a simple solid solution structure. The characteristics of multiple principal elements in high entropy alloys give them lattice distortion effects, thermodynamic high entropy effects, hysteresis diffusion effects of kinetic entropy, and cocktail effects in performance. Traditional high-temperature alloys are widely used in aerospace and other fields. With the proposal of refractory high-entropy alloys by Senkov, the research scope of high-entropy alloys has gradually expanded to high-temperature fields. High-temperature high-entropy alloys are mainly composed of refractory metal elements such as Mo, Ti, V, Nb, Hf, Ta, Cr, and W. They have ultra-high high-temperature strength and are a new type of high-temperature material with potential application prospects.
[0003] However, while traditional refractory high-entropy alloys such as WNbMoTa and WNbMoTaV have high strength, their plasticity is very low. At 1600°C, the compressive strength can reach more than 400MPa, but the room temperature ductility is less than 3%, and the density is high and the fluidity is poor, which makes it difficult to form precision workpieces. Alloys with a compressive strength of more than 400MPa at 2000°C have never been reported. How to design a refractory high-entropy alloy with higher high-temperature strength, better room temperature plasticity, and lower density and cost has become a problem that needs to be solved in the design of high-entropy alloy composition. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present application is to improve the strength of high-temperature refractory high-entropy alloys while solving the problems of high alloy density, poor room temperature plasticity and poor fluidity, and to provide a high-temperature high-entropy alloy containing a eutectic structure and a preparation method thereof.
[0005] To this end, the first technical solution of the present application provides a eutectic high entropy alloy material, which is prepared from the following raw materials in atomic percentage:
[0006] WNbMoTaC: W 23%~27%, Nb 15%~19%, Mo 22%~26%, Ta 15%~19%, C14%~18%; or
[0007] WNbMoC: W 29%-34%, Nb 18%-23%, Mo 29%-33%, C 16%-20%; or
[0008] WNbTaC: W 33%~37%, Nb 22%~26%, Ta 22%~27%, C 14%~18%; or
[0009] WMoTaC: W 28%-33%, Mo 28%-33%, Ta 19%-24%, C 15%-20%; or
[0010] WMoTiC: W 29%-34%, Mo 28%-33%, Ti 20%-24%, C 14%-18%; or
[0011] WTaTiC: W 32%~38%, Ta 22%~27%, Ti 23%~27%, C 12%~16%; or
[0012] WNbTaTiC: W 25%~31%, Nb 17%~21%, Ta 17%~22%, Ti 17%~22%, C11%~16%; or
[0013] WMoTaTiC: 23% ~ 27%, Mo 22% ~ 27%, Ta 16% ~ 19%, Ti 16% ~ 19%, C 13% ~ 16%.
[0014] The above alloys have better fluidity and lower density and can be used in the field of high temperature resistant materials, such as the aerospace field.
[0015] The second technical solution of the present application provides a method for preparing the above-mentioned eutectic high entropy alloy material, comprising the following steps:
[0016] The alloy is obtained by melting the above alloy raw materials in a melting furnace according to their melting points from low to high.
[0017] Preferably, among the raw materials, the C element is introduced as WC as a C source, and the rest are pure elemental raw materials with a purity of 99.99wt%.
[0018] Preferably, the melting furnace is a non-consumable vacuum arc melting furnace, the melting current is 400-500A, the melting voltage is 12V, the melting alloy is kept in liquid state for not less than 3 minutes, one cycle is followed by 6-8 cycles in total.
[0019] Preferably, magnetic stirring is turned on during the 3rd and 4th cycles.
[0020] And, the WNbMoTaTiC series high temperature high entropy alloy containing eutectic material prepared according to the above preparation method.
[0021] The beneficial effects of the present invention over the prior art are as follows: the WNbMoTaTiC eutectic high entropy alloy of the present invention is mainly prepared by a vacuum non-consumable arc melting furnace using a combination of six elements, namely, W, Nb, Mo, Ta, Ti, and C. The eutectic high entropy alloy has better fluidity than other high-temperature refractory alloys. The XRD spectrum shows that the WNbMoTaTiC series high entropy alloy is a BCC, FCC, HCP two-phase or three-phase structure, which is a completely eutectic organization. Due to the narrow solidification range of the eutectic alloy, the alloy of the present invention has excellent casting performance and effectively reduces the generation of hot cracks.
[0022] The WNbMoTaTiC eutectic high entropy alloy of the present invention has higher room temperature strength and better room temperature plasticity than other refractory alloys, while retaining higher ultra-high temperature performance. Its room temperature yield strength can reach up to 2590MPa, with an elongation after fracture greater than 10%, and its yield strength can reach 575MPa at 2000°C.
[0023] The WNbMoTaTiC eutectic high entropy alloy of the present invention has lower density and price than other commercial ultra-high temperature alloys. The alloy density of the present invention is less than 15g / cm 3 The price is less than 2000 yuan / kg. The eutectic refractory high entropy alloy of the present invention has simple preparation process, excellent performance, low cost and good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 W calculated in Example 3 of the present invention 35.5 Nb 24 Ta 24 C 16.5 Solidification path of eutectic high entropy alloys;
[0025] Figure 2 Ta calculated for the present invention 25.5 Nb 25.5 Mo 36 C 13 Solidification path of eutectic high entropy alloys;
[0026] Figure 3 X-ray diffraction (XRD) patterns of the WNbMoTaTiC eutectic high entropy alloys prepared in Examples 1 to 4 of the present invention;
[0027] Figure 4 X-ray diffraction (XRD) patterns of the WNbMoTaTiC eutectic high entropy alloys prepared in Examples 5 to 8 of the present invention;
[0028] Figure 5 W prepared in Example 1 of the present invention 25 Nb17 Mo 24.5 Ta 17 C 16.5 BSE image of eutectic high entropy alloy;
[0029] Figure 6 W prepared in Example 2 of the present invention 31 Nb 21 Mo 30 C 18 BSE image of eutectic high entropy alloy;
[0030] Figure 7 W prepared in Example 3 of the present invention 35.5 Nb 24 Ta 24 C 16.5 BSE image of eutectic high entropy alloy;
[0031] Figure 8 W prepared in Example 4 of the present invention 31 Mo 30 Ta 21 C 18 BSE image of eutectic high entropy alloy;
[0032] Fig. 9 W prepared in Example 5 of the present invention 31 Mo 31 Ti 22 C 16 BSE image of eutectic high entropy alloy;
[0033] Fig.10 W prepared in Example 6 of the present invention 36 Ta 25 Ti 25 C 14 BSE image of eutectic high entropy alloy;
[0034] Fig.11 W prepared in Example 7 of the present invention 28 Nb 19 Ta 20 Ti 20 C 13 BSE image of eutectic high entropy alloy;
[0035] Fig.12 W prepared in Example 8 of the present invention 25 Mo 24.5 Ta 17.5 Ti 18 C 15 BSE image of eutectic high entropy alloy;
[0036] Fig.13This is a BSE picture of the Ta10W high temperature alloy prepared in Comparative Example 1 of the present invention;
[0037] Fig.14 The room temperature compressive stress-strain curves of Example 1, Example 2, Example 3, and Example 6 of the present invention;
[0038] Fig.15 2000°C high temperature compressive stress-strain curves of Example 3 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the present application. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be considered as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so that once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0041] The first embodiment of the present application provides a specific method for screening alloys. The alloys described in the present application are screened by the following ideas.
[0042] S1. Confirm the elements that form eutectic: First, five refractory elements W, Nb, Mo, Ta, and Ti are selected. The difference in mixing enthalpy between each element is small, so we introduce elements with relatively negative mixing enthalpy with the five refractory elements. Non-metallic elements include C, B, Si and other elements, and metal elements include Al, Ni and other elements. Considering the high temperature performance of the alloy, low melting point elements are excluded. Based on experimental experience, we finally confirm that element C is the eutectic element. The addition of element C can make the alloy have a second phase carbide strengthening phase, and the alloy matrix is a BCC solid solution phase formed by the refractory elements W, Nb, Mo, Ta, and Ti.
[0043] The second step is to confirm the eutectic composition through the binary phase diagram between C element and refractory element. Since the mixing enthalpy between C element and refractory element is also different, in order to balance the difference in mixing enthalpy in the alloy, coefficients ɑ, β, and γ are used to balance the composition. The final alloy composition is given by formula 1: C basic =α[Eu(A-B1)]+β[Eu(A-B2)]+γ[Eu(A-B3)], where the coefficients are calculated by formula 2: αΔH A-B1 =βΔH A-B2 =γΔH A-B3 We get: A is the C element, B is the refractory element, Eu(AB) is the eutectic composition, ΔH A-B is the mixing enthalpy between A and B. A large number of theoretical eutectic compositions can be obtained through the second step.
[0044] The third step is to use Thermo-Calc to calculate the solidification path of the theoretical composition, and to filter out the components that do not undergo eutectic reaction through the solidification path to obtain the theoretical composition that can actually form a complete eutectic. For example, in some specific embodiments, the W described in Example 3 is screened out. 35.5 Nb 24 Ta 24 C 16.5 Alloy (such as Figure 1 As shown in Figure 2, the solidification path is calculated: eutectic reaction can occur at around 2750°C, and the liquid phase solidifies into BCC phase and HCP phase at the same time, while for example Ta 25.5 Nb 25.5 Mo 36 C 13 Alloy (such as Figure 2 As shown in the figure, the solidification path is calculated: when the liquid phase is the same as the HCP at about 2500℃, it decreases to produce BCC phase and FCC phase, which is not a eutectic reaction, so the alloy is screened out.
[0045] Through the above method, the specific implementation method of the present application screened out eight WNbMoTaTiC eutectic high entropy alloy materials with ultra-high strength, wherein the first WNbMoTaC eutectic high entropy alloy material is composed of W 23%-27%, Nb 15%-19%, Mo 22%-26%, Ta 15%-19%, and C 14%-18%; the second WNbMoC eutectic high entropy alloy material is composed of W 29%-34%, Nb 18%-23%, Mo 29%-33%, and C 16%-20%; the third WNbTaC eutectic high entropy alloy material is composed of W 33%-37%, Nb 22%-26%, Ta 22%-27%, and C 14%-18%; the fourth WMoTaC eutectic high entropy alloy material is composed of W 28%-33%, Mo 29%-33%, and C 16%-20% by atomic percentage. The fifth WMoTiC eutectic high entropy alloy material has an atomic percentage composition of W 29%-34%, Mo 28%-33%, Ti 20%-24%, and C 14%-18%; the sixth WTaTiC eutectic high entropy alloy material has an atomic percentage composition of W 32%-38%, Ta 22%-27%, Ti 23%-27%, and C 12%-16%; the seventh WNbTaTiC eutectic high entropy alloy material has an atomic percentage composition of W 25%-31%, Nb 17%-21%, Ta 17%-22%, Ti 17%-22%, and C 11%-16%; the eighth WMoTaTiC eutectic high entropy alloy material has an atomic percentage composition of W 23%-27%, Mo 22%-27%, Ta 16%~19%, Ti 16%~19%, C 13%~16%.
[0046] All the alloy components screened above can undergo eutectic reaction.
[0047] The second embodiment of the present application provides a method for preparing an alloy
[0048] S1. Select bulk raw materials of five elements, namely W, Nb, Mo, Ta and Ti, and select WC particles as a C source to introduce the C element, and the purity of the raw materials used is 99.99wt.%; accurately weigh the raw materials of W, Nb, Mo, Ta, Ti and WC according to the atomic percentage of the WNbMoTaTiC eutectic high entropy alloy selected above, wherein the weight of WC is calculated from the mass of C atoms, and the added pure element W is the mass of W remaining after removing the W content in WC, and the accuracy of the balance used is 0.1mg. After the ingredients are prepared, the raw materials are cleaned with an ultrasonic cleaner, and then placed in a copper crucible of a non-consumable vacuum arc melting furnace in the order of the melting points of the raw materials from low to high, i.e., Ti, Nb, Mo, WC, Ta and W;
[0049] Step 2: Close the furnace door and evacuate the non-consumable vacuum arc melting furnace to a vacuum state. The vacuum degree of the furnace is less than 2.5×10 -3 Pa; then high-purity argon gas with a purity of 99.99wt.% is introduced as a protective gas, and the protective atmosphere pressure is 0.05MPa;
[0050] Step 3: First, the pure Ti ingot in the non-consumable vacuum arc melting furnace is melted to reduce the oxygen content in the vacuum chamber. The melting time is 2 minutes, the melting current is about 300A, and the voltage is 12V; then, the raw materials of the WNbMoTaTiC eutectic high entropy alloy are melted for 5 minutes, and then the alloy is kept in liquid for not less than 3 minutes. The melting current is 400-500A and the melting voltage is 12V; after the mother alloy button ingot is cooled, the mother alloy is turned over by a manipulator, and the next melting is carried out by the same method, and a total of six to eight meltings are carried out; among them, magnetic stirring needs to be turned on during the third to fourth melting to make the high entropy alloy mother alloy ingot more uniform. After cooling, a WNbMoTaTiC eutectic high entropy alloy with uniform structure is obtained.
[0051] The following are specific examples.
[0052] Example 1
[0053] This embodiment is a cast W 25 Nb 17 Mo 24.5 Ta 17 C 16.5 The eutectic high entropy alloy has a W, Nb, Mo, Ta, and C atomic percentage of 25%, 17%, 24.5%, 17%, and 16.5% respectively. The purity of the W, Nb, Mo, Ta, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0054] According to W 25 Nb 17 Mo 24.5Ta 17 C 16.5 The atomic percentage of the eutectic high entropy alloy is accurately weighed. The five raw materials of W, Nb, Mo, Ta, and WC are removed from the surface oxide scale with a small grinding wheel and cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Nb, Mo, WC, Ta, and W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0055] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 25 Nb 17 Mo 24.5 Ta 17 C 16.5 The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 25 Nb 17 Mo 24.5 Ta 17 C 16.5 Eutectic high entropy alloy.
[0056] The obtained master alloy ingot was then wire-cut, and 1 mm thick slices were cut along the radius of the alloy ingot to observe the microstructure of different solidification rate areas of the alloy ingot; 10 mm diameter slices were cut for XRD testing to detect the crystal structure; five small cylinders with a diameter of 3.6 mm and a height of 5.4 mm were cut for room temperature compression performance testing.
[0057] To W 25 Nb 17 Mo 24.5 Ta 17 C 16.5 The eutectic high entropy alloy was tested for phase, and the XRD test results were as follows: Figure 3 As shown, combined Figure 5From the backscattered electron image, it can be seen that the high entropy alloy structure of this example is a BCC+FCC two-phase eutectic structure, the FCC phase is carbide MC, and the M elements are Nb and Ta. Fig.14 As shown in the figure, due to its extremely fine eutectic layer and hard carbide, the alloy of this example has high strength, its room temperature compressive yield strength is 2270MPa, and its plasticity is 13.9%. The theoretical density of the alloy of this example is calculated to be 12.78g / cm 3 The cost price is 1733 yuan / kg. Because the eutectic structure has good fluidity, it has a microstructure with fewer defects compared with comparative example 1, and also has a lower density and price.
[0058] Example 2
[0059] This embodiment is a W 31 Nb 21 Mo 30 C 18 The eutectic high entropy alloy has a W, Nb, Mo, and C atomic percentage of 31%, 21%, 30%, and 18% respectively. The purity of the W, Nb, Mo, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0060] According to W 31 Nb 21 Mo 30 C 18 The atomic percentage of eutectic high entropy alloy is accurately weighed. The surface oxide scale of the raw materials is removed with a small grinding wheel, and then the raw materials are cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Nb, Mo, WC, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0061] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 31 Nb 21 Mo 30 C 18The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 31 Nb 21 Mo 30 C 18 Eutectic high entropy alloy.
[0062] The obtained master alloy ingot was then wire-cut, and 1 mm thick slices were cut along the radius of the alloy ingot to observe the microstructure of different solidification rate areas of the alloy ingot; 10 mm diameter slices were cut for XRD testing to detect the crystal structure; five small cylinders with a diameter of 3.6 mm and a height of 5.4 mm were cut for room temperature compression performance testing.
[0063] W 31 Nb 21 Mo 30 C 18 The XRD test results of eutectic high entropy alloy are as follows: Figure 3 As shown, it is a three-phase structure of BCC+HCP+FCC, combined with Figure 6 From the backscattered electron image, we can see that the unstable M2C will partially decompose into MC with FCC crystal structure, where M represents Nb and Ta elements, so some very fine lamellar structures can be observed in the microstructure. Due to its very fine eutectic layer and hard carbides, the alloy in this example has high strength. The room temperature compression performance is as follows Fig.14 As shown, the room temperature compressive yield strength of the alloy in this example is 2268MPa, and the plasticity is 10.9%. The theoretical density of the alloy in this example is calculated to be 11.94g / cm 3 The cost price is 991 yuan / kg. Because the eutectic structure has good fluidity, it has a microstructure with fewer defects compared with Comparative Example 1, and also has a lower density and price.
[0064] Example 3
[0065] This embodiment is a cast W 35.5 Nb 24 Ta 24 C 16.5 The eutectic high entropy alloy has a W, Nb, Ta, and C atomic percentage of 35.5%, 24%, 24%, and 16.5% respectively. The purity of the W, Nb, Ta, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0066] According to W 35.5 Nb 24 Ta 24 C 16.5 The atomic percentage of eutectic high entropy alloy is accurately weighed. The surface oxide scale of the raw materials is removed with a small grinding wheel, and then the raw materials are cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Nb, WC, Ta, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0067] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 35.5 Nb 24 Ta 24 C 16.5 The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 35.5 Nb 24 Ta 24 C 16.5 Eutectic high entropy alloy.
[0068] Subsequently, the obtained mother alloy ingot was wire-cut, and 1 mm thick slices were cut along the radius of the alloy ingot to observe the microstructure of different solidification rate areas of the alloy ingot; 10 mm diameter slices were cut for XRD testing to detect the crystal structure; five small cylinders with a diameter of 3.6 mm and a height of 5.4 mm were cut for room temperature compression performance testing, and two small cylinders with a diameter of 3.6 mm and a height of 5.4 mm were cut for 2000°C high temperature compression performance testing.
[0069] W 35.5 Nb 24 Ta 24 C 16.5 The XRD test results of eutectic high entropy alloy are as follows: Figure 3 As shown, combined Figure 7 From the backscattered electron image, it can be seen that the alloy structure of this embodiment is a two-phase eutectic structure of BCC+HCP, and the HCP phase is carbide M2C, where M is Nb and Ta elements. Fig.14 As shown, the room temperature compressive yield strength of the alloy of this example is 2590MPa, and the plasticity is 11.5%. The 2000℃ high temperature compressive performance of this example is as follows Fig.15 As shown, the high temperature compressive yield strength is 575MPa. The calculated theoretical density is 14.02g / cm 3 , the cost price is 1937 yuan / kg. Compared with comparative example 1, due to the characteristics of eutectic structure, the microstructure is uniform, dense and defect-free, and the high temperature strength is almost 10 times that of comparative example 1. At the same time, it has lower density and price, and has a higher application prospect.
[0070] Example 4
[0071] This embodiment is a cast W 31 Mo 30 Ta 21 C 18 The eutectic high entropy alloy has a W, Mo, Ta, and C atomic percentage of 31%, 30%, 21%, and 18% respectively. The purity of the W, Mo, Ta, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0072] According to W 31 Mo 30 Ta 21 C 18 The atomic percentage of eutectic high entropy alloy is accurately weighed. The surface oxide scale of the raw materials is removed with a small grinding wheel, and then the raw materials are cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Mo, WC, Ta, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0073] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 31 Mo 30 Ta 21 C 18The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 31 Mo 30 Ta 21 C 18 Eutectic high entropy alloy.
[0074] The obtained master alloy ingot was then wire cut, and a 1 mm thick slice was cut along the radius of the alloy ingot to observe the microstructure of the alloy ingot in different solidification rate areas; a 10 mm diameter slice was cut for XRD testing to detect the crystal structure.
[0075] To W 31 Mo 30 Ta 21 C 18 The eutectic high entropy alloy was tested for phase, and the XRD test results were as follows: Figure 3 As shown, combined Figure 8 From the backscattered electron image, we can see that the high entropy alloy structure of this example is a BCC+HCP two-phase eutectic structure, the BCC phase is carbide M2C, where the M elements are Nb and Ta. The theoretical density of the alloy in this example is calculated to be 14.01g / cm 3 The cost price is 1836 yuan / kg. Because the eutectic structure has good fluidity, it has a microstructure with fewer defects compared with comparative example 1, and also has a lower density and price.
[0076] Example 5
[0077] This embodiment is a cast W 31 Mo 31 Ti 22 C 16 The eutectic high entropy alloy has a W, Mo, Ti, and C atomic percentage of 31%, 31%, 22%, and 16% respectively. The purity of the W, Mo, Ti, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0078] According to W 31 Mo 31 Ti 22 C 16The atomic percentage of eutectic high entropy alloy is accurately weighed. The surface oxide scale of the raw materials is removed with a small grinding wheel, and then the raw materials are cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Ti, Mo, WC, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0079] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 31 Mo 31 Ti 22 C 16 The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 31 Mo 31 Ti 22 C 16 Eutectic high entropy alloy.
[0080] The obtained master alloy ingot was then wire cut, and a 1 mm thick slice was cut along the radius of the alloy ingot to observe the microstructure of the alloy ingot in different solidification rate areas; a 10 mm diameter slice was cut for XRD testing to detect the crystal structure.
[0081] To W 31 Mo 31 Ti 22 C 16 The eutectic high entropy alloy was tested for phase, and the XRD test results were as follows: Figure 4 As shown, combined Fig. 9 From the backscattered electron image, we can see that the high entropy alloy structure of this example is a BCC+FCC two-phase eutectic structure, the FCC phase is carbide MC, and the M element is mainly Ti. The theoretical density of the alloy in this example is calculated to be 10.98g / cm 3The cost price is 902 yuan / kg. Because the addition of Ti element, the alloy has lower density and price. Because the eutectic structure has good fluidity, it has a microstructure with fewer defects compared with comparative example 1, and also has lower density and price.
[0082] Example 6
[0083] This embodiment is a cast W 36 Ta 25 Ti 25 C 14 The eutectic high entropy alloy has a W, Ta, Ti, and C atomic percentage of 36%, 25%, 25%, and 14% respectively. The purity of the W, Ta, Ti, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0084] According to W 36 Ta 25 Ti 25 C 14 The atomic percentage of eutectic high entropy alloy is accurately weighed. The surface oxide scale of the raw materials is removed with a small grinding wheel, and then the raw materials are cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Ti, WC, Ta, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0085] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 36 Ta 25 Ti 25 C 14 The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 36 Ta 25 Ti 25 C14 Eutectic high entropy alloy.
[0086] The obtained master alloy ingot was then wire-cut, and 1 mm thick slices were cut along the radius of the alloy ingot to observe the microstructure of different solidification rate areas of the alloy ingot; 10 mm diameter slices were cut for XRD testing to detect the crystal structure; five small cylinders with a diameter of 3.6 mm and a height of 5.4 mm were cut for room temperature compression performance testing.
[0087] To W 36 Ta 25 Ti 25 C 14 The eutectic high entropy alloy was tested for phase, and the XRD test results were as follows: Figure 4 As shown, combined Fig.10 From the backscattered electron image, it can be seen that the high entropy alloy structure of this example is a BCC+FCC two-phase eutectic structure, the FCC phase is carbide MC, and the M elements are Ti and Ta. Fig.14 As shown in the figure, due to its extremely fine eutectic layer and hard carbide, the alloy of this example has high strength, its room temperature compressive yield strength is 2107MPa, and its plasticity is 11.2%. The theoretical density of the alloy of this example is calculated to be 13.02g / cm 3 The cost price is 1939 yuan / kg. Because the eutectic structure has good fluidity, it has a microstructure with fewer defects compared with comparative example 1, and also has a lower density and price.
[0088] Example 7
[0089] This embodiment is a cast W 28 Nb 19 Ta 20 Ti 20 C 13 The eutectic high entropy alloy has a composition of W, Nb, Ta, Ti, and C in atomic percentages of 28%, 19%, 20%, 20%, and 13%, respectively. The purity of the W, Nb, Ta, Ti, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0090] According to W 28 Nb 19 Ta 20 Ti 20 C 13The atomic percentage of the eutectic high entropy alloy is accurately weighed. The surface oxide scale of the raw materials is removed with a small grinding wheel, and then the raw materials are cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Ti, Nb, WC, Ta, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0091] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 28 Nb 19 Ta 20 Ti 20 C 13 The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 28 Nb 19 Ta 20 Ti 20 C 13 Eutectic high entropy alloy.
[0092] The obtained master alloy ingot was then wire cut, and a 1 mm thick slice was cut along the radius of the alloy ingot to observe the microstructure of the alloy ingot in different solidification rate areas; a 10 mm diameter slice was cut for XRD testing to detect the crystal structure.
[0093] To W 28 Nb 19 Ta 20 Ti 20 C 13 The eutectic high entropy alloy was tested for phase, and the XRD test results were as follows: Figure 4 As shown, combined Fig.11From the backscattered electron image, we can see that the high entropy alloy structure of this example is a three-phase eutectic structure of BCC+BCC#2+FCC, and the FCC phase is carbide MC, where the M elements are Nb, Ta, and Ti. The theoretical density of the alloy in this example is calculated to be 11.94g / cm 3 The cost price is 1806 yuan / kg. Because the eutectic structure has good fluidity, it has a microstructure with fewer defects compared with comparative example 1, and also has a lower density and price.
[0094] Example 8
[0095] This embodiment is a cast W 25 Mo 24.5 Ta 17.5 Ti 18 C 15 The eutectic high entropy alloy has a W, Mo, Ta, Ti, and C atomic percentage of 25%, 24.5%, 17.5%, 18%, and 15% respectively. The purity of the W, Mo, Ta, Ti, and WC raw materials is higher than 99.99wt.%. The specific preparation method is:
[0096] According to W 25 Mo 24.5 Ta 17.5 Ti 18 C 15 The atomic percentage of the eutectic high entropy alloy is accurately weighed. The surface oxide scale of the raw materials is removed with a small grinding wheel, and then the raw materials are cleaned with an ultrasonic cleaner. The mass of WC is calculated according to the amount of C element added, and the remaining W is supplemented with single W element. The prepared metal raw materials are ultrasonically cleaned separately. According to the order of the melting point of the raw materials from low to high, that is, Ti, Mo, WC, Ta, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0097] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, W 25 Mo 24.5 Ta 17.5 Ti 18 C 15The raw materials of the eutectic high entropy alloy are melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain a mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain W 25 Mo 24.5 Ta 17.5 Ti 18 C 15 Eutectic high entropy alloy.
[0098] The obtained master alloy ingot was then wire cut, and a 1 mm thick slice was cut along the radius of the alloy ingot to observe the microstructure of the alloy ingot in different solidification rate areas; a 10 mm diameter slice was cut for XRD testing to detect the crystal structure.
[0099] To W 25 Mo 24.5 Ta 17.5 Ti 18 C 15 The eutectic high entropy alloy was tested for phase, and the XRD test results were as follows: Figure 4 As shown, combined Fig.12 From the backscattered electron image, we can see that the high entropy alloy structure of this example is a BCC+FCC two-phase eutectic structure, the FCC phase is carbide MC, and the M elements are Ti and Ta. The theoretical density of the alloy in this example is calculated to be 12.05g / cm 3 The cost price is 1721 yuan / kg. Because the eutectic structure has good fluidity, it has a microstructure with fewer defects compared with comparative example 1, and also has a lower density and price.
[0100] Comparative Example 1
[0101] This comparative example is a commercial Ta10W high temperature alloy, the atomic percentages of the constituent elements W and Ta are 10% and 90% respectively. The purity of the W and Ta metal raw materials is higher than 99.99wt.%. In this comparative example, the same preparation method as in the above embodiment is adopted, and the specific preparation method is:
[0102] Select two pure metal raw materials, W and Ta, remove the surface oxide scale of the raw materials with a small grinding wheel, and use an ultrasonic cleaner to clean them. Accurately weigh the two metal raw materials W and Ta according to the atomic percentage of Ta10W high-temperature alloy. Ultrasonic clean the prepared metal raw materials respectively. According to the order of the melting point of the raw materials from low to high, that is, Ta, W, the metal raw materials are placed in the copper crucible of the vacuum arc melting furnace in sequence.
[0103] Then close the door of the vacuum melting furnace and evacuate the furnace chamber to a high vacuum state, with a vacuum degree of no more than 2.5×10 -3 Pa. Then, high-purity argon gas with a purity greater than 99.99wt.% is introduced as a protective gas, and the furnace chamber pressure is set to 0.05MPa. First, the titanium block is melted to consume the residual oxygen. The melting time is 2min, the current is about 300A, and the voltage is about 12V. Then, the raw material of the Ta10W high-temperature alloy is melted, the melting current is 450A, the melting voltage is about 12V, and the melting time is about 5min. Wait until the metal is completely solidified and cooled to obtain the mother alloy button ingot. The mother alloy ingot is turned over by a manipulator, and the same method is used for the next melting, for a total of six meltings. Among them, from the third to the fourth melting, it is necessary to turn on the magnetic stirring to make the high-entropy alloy mother alloy ingot more uniform, and the magnetic stirring current is maintained at about 10A. After the melting is completed, wait until the copper mold cools to room temperature, open the furnace door, take out the sample, and obtain the Ta10W high-temperature alloy.
[0104] The obtained mother alloy ingot was then wire-cut, and thin slices with a thickness of 1 mm were cut along the radius of the alloy ingot to observe the microstructure of the alloy ingot in different solidification rate areas, and compared with the three embodiments described above; two small cylinders with a diameter of 3.6 mm and a height of 5.4 mm were cut for 2000°C high-temperature compression performance test, and compared with Example 3.
[0105] Backscattered electron images of Ta10W superalloy Fig.13 As shown in Figure 1, it is a single-phase structure, and the smelted structure has more pores; the high-temperature compression performance at 2000℃ is shown in Figure 1. Fig.15 As shown, the high temperature compressive yield strength is 59MPa, and no fracture occurs under compression. Its theoretical density is 16.92g / cm 3 The cost price is 3516 yuan / kg. Compared with this commercial high-temperature alloy, the embodiment of this patent has better high-temperature performance, lower density and price, and has good application prospects.
[0106] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. Eutectic high entropy alloy material, characterized in that: It is prepared from the following raw materials in atomic percentage: WNbMoTaC: W 23% ~ 27%, Nb 15% ~ 19%, Mo 22% ~ 26%, Ta 15% ~ 19%, C 14% ~ 18%; or WNbMoC: W 29% ~ 34%, Nb 18% ~ 23%, Mo 29% ~ 33%, C 16% ~ 20%; or WNbTaC: W 33%~37%, Nb 22%~26%, Ta 22%~27%, C 14%~18%; or WMoTaC: W 28%-33%, Mo 28%-33%, Ta 19%-24%, C 15%-20%; or WMoTiC: W 29%-34%, Mo 28%-33%, Ti 20%-24%, C 14%-18%; or WTaTiC: W 32%~38%, Ta 22%~27%, Ti 23%~27%, C 12%~16%; or WNbTaTiC: W 25%~31%, Nb 17%~21%, Ta 17%~22%, Ti 17%~22%, C 11%~16%; or WMoTaTiC: 23% ~ 27%, Mo 22% ~ 27%, Ta 16% ~ 19%, Ti 16% ~ 19%, C 13% ~ 16%.
2. Application of the eutectic high entropy alloy according to claim 1 in the field of high temperature resistant materials.
3. A method for preparing the eutectic high entropy alloy material as claimed in claim 1, characterized in that: The steps include: The raw materials described in claim 1 are placed in a smelting furnace and smelted according to their melting points from low to high.
4. The preparation method according to claim 3, characterized in that: Among the raw materials, the C element is introduced as WC as a C source, and the rest are pure elemental raw materials with a purity of 99.99wt%.
5. The preparation method according to claim 4, characterized in that: The melting furnace is a non-consumable vacuum arc melting furnace, the melting current is 400-500A, the melting voltage is 12V, the melting alloy is kept in liquid state for not less than 3 minutes, one cycle is followed, and 6-8 cycles are performed in total.
6. The preparation method according to claim 5, characterized in that: Magnetic stirring was turned on during the 3rd and 4th cycles.
7. A eutectic high entropy alloy prepared according to any one of the preparation methods of claims 3-6.
Citation Information
Patent Citations
Low-density biphase silicide reinforced refractory high-entropy alloy and preparation method thereof
CN113584368A
In-situ generated carbide enhanced Nb-Mo-Ta-W-M-C high-temperature eutectic high-entropy alloy and preparation method thereof
CN116891969A
Refractory high-entropy alloy with ultrahigh-temperature strength and preparation method of refractory high-entropy alloy
CN117488164A
Lightweight high-entropy alloy having high strength and high plasticity and preparation method therefor
WO2020118802A1
Cited By
High-temperature-resistant eutectic high-entropy alloy and preparation method and application thereof
CN120158665A