Austenitic stainless steel with small welding slag generation amount during pipe welding and preparation method of austenitic stainless steel

By controlling the composition and welding process of inclusions in austenitic stainless steel, the melting point of inclusions is reduced, and the problem of large amount of welding slag generation in welding pipes is solved, and the quality and corrosion resistance of welds are improved. It is suitable for commonly used 304, 316 grade stainless steel.

CN119061316AInactive Publication Date: 2024-12-03ZHANGJIAGANG POHANG STAINLESS STEEL
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411523301.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the welding pipe making process of austenitic stainless steel, the amount of welding slag is generated relatively large, which affects the quality and corrosion resistance of welds. The prior art methods such as CN102308012A have limitations when applied to commonly used 304 and 316 grade stainless steels.

Method used

By controlling the composition of inclusions in austenitic stainless steel, MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, SiO2: 32.0-66.0%, the rest are other inevitable oxides, and MgAl2O4, CaO, SiO2, three The total components of the inclusions account for 82 to 95% of the total inclusions, so as to reduce the melting point of the inclusions, make them easy to melt during welding, and reduce the generation of welding slag. The specific processes include melting and refining in the EAF furnace and the AOD furnace, deoxygenation using low aluminum-ferrosilicon alloy, controlling alkalinity and steel outlet temperature, and continuous casting in the dolomite ladle, always passing protective gas to prevent oxide formation.

Benefits of technology

Effectively reduce the generation of welding slag during welding pipe making, improve the quality and corrosion resistance of welds, and is suitable for commonly used grade 304 and 316 stainless steels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061316A_ABST
    Figure CN119061316A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of austenitic stainless steel with less welding slag generation during pipe welding. The preparation method comprises the following steps: (1) raw materials are put into an EAF furnace for melting; pre-desulfurizing before tapping; (2) the AOD furnace refining process comprises the steps of oxygen blowing decarburization, reduction and tapping; wherein in the reduction process, a low-aluminum ferrosilicon alloy is adopted for deoxidation, the input amount of the low-aluminum ferrosilicon alloy is 20-35 kg / ton, the silicon content in the low-aluminum ferrosilicon alloy is 75-80%, and the aluminum content in the low-aluminum ferrosilicon alloy is 0.5% or below; in the whole AOD refining process, the alkalinity of the refining slag is controlled to be 1.7 + / -0.1; in the tapping process, the tapping temperature is controlled to be 1625 + / -25 DEG C; (3) molten steel refined in the AOD furnace is poured into a dolomite steel ladle; and (4) continuous casting: the molten steel in the dolomite steel ladle enters a continuous casting machine for continuous casting through a tundish. The method has the advantage that the welding slag generation amount is small during pipe welding and manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of austenitic stainless steel, and in particular to a method for preparing austenitic stainless steel with less welding slag generated during welding pipe making. Background Art

[0002] When austenitic stainless steel is used for welding pipe making, austenitic stainless steel strips with a thickness of less than 2.0 mm are usually manufactured by self-melting argon arc welding (TIG) welding method, that is, TIG welding provides heat, no welding wire is added during welding, and the weld is obtained only by melting the butt joint of the stainless steel strip and solidifying it, so that the stainless steel strips are butted to form a welded pipe.

[0003] During the welding process, welding slag will be formed on the weld surface (inside / outside). The occurrence of welding slag is due to the fact that the inclusions in the material matrix are not easy to melt during welding. The main components of the inclusions include MgAl2O4, CaO, SiO2, and other inevitable oxides. Under the action of welding convection, they gather and float on the weld surface to form welding slag. Welding slag will affect the quality of the weld and make the weld incomplete. The presence of local impurities will also reduce the corrosion resistance. Under the condition that grinding is allowed, some welding slag will reduce the thickness of the welded pipe wall to below the nominal thickness after complete grinding, affecting the quality of the finished welded pipe. Therefore, the occurrence of welding slag during welding should be reduced as much as possible.

[0004] At present, the invention patent with patent publication number CN102308012A discloses a "ferritic stainless steel with less black spot generation". In this patent, the reduction of black spot generation is achieved by controlling BI=3Al+Ti+0.5Si+200Ca≤0.8. However, since the commonly used 304 and 316 grade stainless steels do not contain the Ti element, they have limitations in the application of austenitic stainless steel. Summary of the invention

[0005] A first object of the present invention is to provide an austenitic stainless steel which generates less slag during pipe making by welding.

[0006] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: an austenitic stainless steel with a small amount of welding slag generated during welding pipe making, characterized in that the composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, SiO2: 32.0-66.0%, and the rest are other inevitable oxides, and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total number of inclusion components.

[0007] A second object of the present invention is to provide a method for producing austenitic stainless steel with a small amount of slag generated during pipe welding.

[0008] To achieve the above object, the present invention adopts the following technical solution: a method for preparing austenitic stainless steel with less slag generated during welding pipe making, comprising the following steps: (1) Put the raw materials into the EAF furnace for melting to form molten steel; pre-desulfurize the molten steel before tapping to control the sulfur content in the molten steel below 0.05%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 20-35 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 75-80%, and the aluminum content of the low aluminum ferrosilicon alloy is less than 0.5%; During the entire AOD refining process, the basicity of the refined slag was controlled at 1.7±0.1; In the steel tapping process, the tapping temperature is controlled at 1625±25°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel. The composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, SiO2: 32.0-66.0%, and the rest are other inevitable oxides, and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total number of inclusion components; before the molten steel is put into the tundish, the air in the tundish is exhausted with a protective gas, and the protective gas is always introduced into the tundish during the entire continuous casting process.

[0009] Furthermore, in the aforementioned method for preparing austenitic stainless steel with a small amount of welding slag generated during welding pipe making, in which: in step (1), the molten steel is pre-desulfurized by adding lime into the molten steel.

[0010] Furthermore, in the aforementioned method for preparing austenitic stainless steel with low slag generation during welding pipe making, in which: in step (2), in the reduction process, when low aluminum silicon ferroalloy is used for deoxidation, the input amount of the low aluminum silicon ferroalloy is 30 kg / ton, the silicon content of the low aluminum silicon ferroalloy is 78%, and the aluminum content of the low aluminum silicon ferroalloy is less than 0.5%.

[0011] Furthermore, in the aforementioned method for preparing austenitic stainless steel with low slag generation during welding pipe making, in step (2), the basicity of the refined slag is controlled at 1.7 during the entire AOD refining process.

[0012] Furthermore, the aforementioned method for preparing austenitic stainless steel with less slag generated during welding pipe making, wherein: in step (2), in the steel tapping process, the steel tapping temperature is controlled at 1625°C.

[0013] Furthermore, in the aforementioned method for preparing austenitic stainless steel with less slag generated during welding pipe making, in step (4), argon is used as the shielding gas.

[0014] Through the implementation of the above technical scheme, the beneficial effects of the present invention are as follows: the main component composition of inclusions in austenitic stainless steel during steelmaking is controlled through the smelting process, and the composition of the three main components of the inclusions, MgAl2O4, CaO, and SiO2, is controlled, thereby effectively reducing the melting point of the inclusions. Since the melting point of the inclusions with the main component composition ratio is low, the inclusions are easily melted and liquid when the austenitic stainless steel is welded to form pipes, so that the inclusions will not gather and float on the weld surface to form welding slag during welding, thereby effectively reducing the generation of welding slag during welding pipe making. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 Schematic diagram of the structure of dolomite ladle.

[0016] Figure 2 Schematic diagram of the structure of the intermediate package. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0018] Austenitic stainless steel with less slag generated during pipe welding, the composition of inclusions in the austenitic stainless steel includes: MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, SiO2: 32.0-66.0%, and the rest are other inevitable oxides, and the sum of the components of MgAl2O4, CaO, and SiO2 accounts for 82-95% of the total number of inclusion components; the present invention controls the melting point of the inclusions by controlling the composition ratio of the three main components MgAl2O4, CaO, and SiO2 in the inclusions. When the composition ratio of the three main components MgAl2O4, CaO, and SiO2 in the inclusions meets the above conditions, the melting point of the inclusions is low, so that the inclusions are easily melted in a liquid state during welding, and then the inclusions will not gather and float on the weld surface to form slag during welding, thereby effectively reducing the generation of slag.

[0019] like Figure 1 , Figure 2 As shown, a method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel; before tapping, the molten steel is pre-desulfurized by adding lime to the molten steel to control the sulfur content in the molten steel to below 0.05%; the purpose of controlling the sulfur content in the molten steel in this EAF process is to facilitate the control and adjustment of the basicity of the refining slag in the subsequent AOD furnace refining process; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 20-35 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 75-80%, and the aluminum content of the low aluminum ferrosilicon alloy is less than 0.5%; During the entire AOD refining process, the basicity of the refined slag was controlled at 1.7±0.1; In the steel tapping process, the steel tapping temperature is controlled at 1625±25°C; low steel tapping temperature can reduce the degree of reaction between Mg and Al in the molten steel and oxygen, so that when the molten steel enters the dolomite ladle, the reaction between Mg and Al in the molten steel and oxygen to generate MgAl2O4 is reduced, and the generation of inclusions MgAl2O4 is reduced; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; Figure 1 As shown, the structure of the dolomite ladle includes: a ladle body 1 with an open top and other closed sides, and a dolomite refractory layer 2 made of dolomite is covered on the inner wall of the ladle body 1; since the dolomite refractory layer 2 in contact with the molten steel in the dolomite ladle does not contain aluminum, the reaction between the refractory layer and the molten steel can be avoided, thereby preventing the increase of the aluminum content in the molten steel, and thus reducing the generation of MgAl2O4 in the inclusions; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel, wherein the composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, SiO2: 32.0-66.0%, and the rest are other inevitable oxides, and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total components of the inclusions; Before the molten steel is put into the tundish, the air in the tundish is exhausted with protective gas, and the protective gas is always introduced into the tundish during the entire continuous casting process. Figure 2As shown, the structure of the tundish includes a tundish body 3 and a cover 4. The top of the tundish body 3 is open, and a discharge port 5 is arranged at the bottom of the tundish body 3. The cover 4 is arranged on the top of the tundish body 3. A feed port 6 and a protective gas inlet 7 are arranged on the cover 4. Before the molten steel is put into the tundish, argon gas is first introduced into the tundish through the protective gas inlet 7 to exhaust the air in the tundish. In the entire continuous casting process, argon gas is always introduced into the tundish through the protective gas inlet 7. In this way, during the continuous casting process, an argon gas gap is always formed between the liquid level of the molten steel 8 in the tundish and the cover 4. The argon protective layer 9 composed of gas is used to isolate the outside air, prevent the invasion of external oxygen, and avoid the reaction of Mg and Al in the molten steel with oxygen to generate MgAl2O4, thereby reducing the generation of inclusions MgAl2O4; the present invention controls the melting point of the inclusions by controlling the composition ratio of the three main components MgAl2O4, CaO, and SiO2 in the inclusions, thereby effectively lowering the melting point of the inclusions, making the inclusions easy to melt in liquid form during welding, and preventing the inclusions from gathering and floating on the weld surface to form welding slag during welding, thereby effectively reducing the generation of welding slag. Example 1

[0020] A method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel. Before tapping, lime is added to the molten steel to pre-desulfurize the molten steel. The sulfur content in the molten steel is 0.023%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 30 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 78%, and the aluminum content of the low aluminum ferrosilicon alloy is 0.25%; During the entire AOD refining process, the basicity of the refined slag was 1.7; In the steel tapping process, the tapping temperature is 1625°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel, wherein the composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 11.6-31%, CaO: 9.9-38%, SiO2: 34.8-53.8%, and the rest are other inevitable oxides; and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total components of the inclusions; wherein, before the molten steel is put into the tundish, the air in the tundish is exhausted with argon gas, and argon gas is always introduced into the tundish during the entire continuous casting process. Example 2

[0021] A method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel. Before tapping, lime is added to the molten steel to pre-desulfurize the molten steel. The sulfur content in the molten steel is 0.048%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 20 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 75%, and the aluminum content of the low aluminum ferrosilicon alloy is 0.49%; During the entire AOD refining process, the basicity of the refined slag was 1.6; In the steel tapping process, the tapping temperature is 1639°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel, wherein the composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 14.0-28.4%, CaO: 19.1-35.4%, SiO2: 32-57.3%, and the rest are other inevitable oxides; and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total components of the inclusions; wherein, before the molten steel is put into the tundish, the air in the tundish is exhausted with argon gas, and argon gas is always introduced into the tundish during the entire continuous casting process. Example 3

[0022] A method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel. Before tapping, lime is added to the molten steel to pre-desulfurize the molten steel. The sulfur content in the molten steel is 0.042%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 35 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 80%, and the aluminum content of the low aluminum ferrosilicon alloy is 0.36%; During the entire AOD refining process, the basicity of the refined slag was 1.67; In the steel tapping process, the tapping temperature is 1650°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel, wherein the composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 8-29.8%, CaO: 9.5-26.9%, SiO2: 42.2-56.1%, and the rest are other inevitable oxides; and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total number of inclusion components; wherein, before the molten steel is put into the tundish, the air in the tundish is exhausted with argon gas, and argon gas is always introduced into the tundish during the entire continuous casting process. Example 4

[0023] A method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel. Before tapping, lime is added to the molten steel to pre-desulfurize the molten steel. The sulfur content in the molten steel is 0.028%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 26 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 77%, and the aluminum content of the low aluminum ferrosilicon alloy is 0.13%; During the entire AOD refining process, the basicity of the refined slag was 1.8; In the steel tapping process, the tapping temperature is 1600°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel, wherein the composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 12.4-29.4%, CaO: 10.5-26.5%, SiO2: 45.3-66%, and the rest are other inevitable oxides; and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total components of the inclusions; wherein, before the molten steel is put into the tundish, the air in the tundish is exhausted with argon gas, and argon gas is always introduced into the tundish during the entire continuous casting process.

[0024] Comparative Example 1 A method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel. Before tapping, lime is added to the molten steel to pre-desulfurize the molten steel. The sulfur content in the molten steel is 0.056%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 18 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 72%, and the aluminum content of the low aluminum ferrosilicon alloy is 0.65%; During the entire AOD refining process, the basicity of the refined slag was 1.89; In the steel tapping process, the tapping temperature is 1688°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel. The composition of the inclusions in the austenitic stainless steel comprises: MgAl2O4: 30.9-79.8%, CaO: 0.5-31.5%, SiO2: 3.0-25.0%, and the rest are other inevitable oxides; before the molten steel is put into the tundish, the air in the tundish is exhausted with argon gas, and argon gas is always introduced into the tundish during the entire continuous casting process.

[0025] Comparative Example 2 A method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel. Before tapping, the molten steel is pre-desulfurized by adding lime to the molten steel, and the sulfur content in the molten steel is 0.11%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 37 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 72%, and the aluminum content of the low aluminum ferrosilicon alloy is 1.3%; During the entire AOD refining process, the basicity of the refined slag was 2.2; In the steel tapping process, the tapping temperature is 1702°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel. The composition of the inclusions in the austenitic stainless steel comprises: MgAl2O4: 7.5-27.8%, CaO: 36.6-64.6%, SiO2: 13.2-26.4%, and the rest are other inevitable oxides; before the molten steel is put into the tundish, the air in the tundish is exhausted with argon gas, and argon gas is always introduced into the tundish during the entire continuous casting process.

[0026] Comparative Example 3 A method for preparing austenitic stainless steel with less slag generated during welding pipe making comprises the following steps: (1) The raw materials are put into the EAF furnace for melting to form molten steel. Before tapping, lime is added to the molten steel to pre-desulfurize the molten steel. The sulfur content in the molten steel is 0.098%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 16 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 72%, and the aluminum content of the low aluminum ferrosilicon alloy is 0.68%; During the entire AOD refining process, the basicity of the refined slag is controlled at 2.1; In the steel tapping process, the tapping temperature is 1695°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously cast into a continuous casting machine through a tundish to form austenitic stainless steel. The composition of the inclusions in the austenitic stainless steel comprises: MgAl2O4: 4.7-20.9%, CaO: 1.1-8.5%, SiO2: 70.4-78.5%, and the rest are other inevitable oxides; before the molten steel is put into the tundish, the air in the tundish is exhausted with argon gas, and argon gas is always introduced into the tundish during the entire continuous casting process.

[0027] The determination method of the inclusion composition in each embodiment and each comparative example of the present invention is a common technology, specifically: sampling the slab after continuous casting and making a metallographic sample with a bright surface through cutting, hot mounting, grinding and polishing, and then using an electron probe (EPMA: Electron Probe Microanalysis) device to scan and analyze the inclusion composition on the polished surface of the sample to obtain the inclusion composition. The present invention continuously collects and analyzes the inclusion composition at multiple different positions of the slab sample through an electronic probe device, thereby obtaining the inclusion composition range.

[0028] Since the slag point of austenitic stainless steel is caused by the presence of high melting point inclusions when using argon arc welding (TIG) to weld pipes, the evaluation of the slag generation can also indirectly reflect the melting point of inclusions in austenitic stainless steel (reference: B. Pollard. The Effect of Minor Elements on the Welding Characteristics of Stainless Stee. Welding Research Supplement (1988), 202-sto 213-s.). The effectiveness of inclusion control is evaluated based on the amount of slag point generated per 6 meters of welded pipe.

[0029] Since the composition of inclusions at various positions in austenitic stainless steel is not consistent, when characterizing the inclusion composition of austenitic stainless steel, it can only be characterized by the range of each component of the inclusions. The inclusion composition ranges of the embodiments and comparative examples of the present invention are obtained by collecting and analyzing the inclusion composition at multiple points of austenitic stainless steel using an electronic probe device. Since there are many actual collection points, the embodiments and comparative examples of the present invention only select the inclusion composition collected at a few points. The present invention lists the inclusion composition collected at three to six points selected in embodiments 1 to 4 and comparative examples 1 to 3 and the corresponding slag generation in Table 1 below:

[0030] From the above examples and comparative data, it can be seen that the main components of the inclusions in the austenitic stainless steel obtained in Examples 1 to 4 are controlled within the range of: MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, SiO2: 32.0-66.0%, and the sum of the components of MgAl2O4, CaO, and SiO2 accounts for 82-95% of the total number of the inclusion components. Within this composition range, the amount of welding slag points generated per 6 meters of welded pipe is 0 or 1, which indirectly reflects that the melting point of the inclusions in the austenitic stainless steel obtained in Examples 1 to 4 is low; The amount of welding slag points generated in the austenitic stainless steel prepared in Comparative Examples 1 to 3 per 6-meter welded pipe is 6 to 12, which is much higher than the amount of welding slag points generated in Examples 1 to 4, which indirectly reflects that the melting point of inclusions in the austenitic stainless steel prepared in Comparative Examples 1 to 3 is high.

[0031] The invention has the advantages that the main component composition of inclusions in austenitic stainless steel during steelmaking is controlled by a smelting process, and the main component composition of the inclusions MgAl2O4, CaO and SiO2 is controlled within the range of MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, and SiO2: 32.0-66.0%, and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total number of the inclusion components, thereby effectively reducing the melting point of the inclusions. Since the melting point of the inclusions with the main component composition ratio is low, the inclusions are easily melted and liquid when the austenitic stainless steel is welded to form pipes, so that the inclusions will not gather and float on the weld surface to form welding slag during welding, thereby effectively reducing the amount of welding slag generated during welding pipe making.

[0032] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.

Claims

1. Austenitic stainless steel with low slag generation during pipe welding, characterized by: The composition of inclusions in austenitic stainless steel includes: MgAl2O4: 8.0~31.0%, CaO: 9.5~38.0%, SiO2: 32.0~66.0%, and the rest are other inevitable oxides. Moreover, the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82~95% of the total inclusion components.

2. A method for preparing austenitic stainless steel with less slag generated during welding pipe making, characterized in that: The following steps are involved: (1) Put the raw materials into the EAF furnace for melting to form molten steel; pre-desulfurize the molten steel before tapping to control the sulfur content in the molten steel below 0.05%; (2) The molten steel after the initial refining in the EAF furnace is put into the AOD furnace for refining. The refining process of the AOD furnace includes: oxygen blowing decarburization → reduction → steel tapping; among which: In the reduction process, low aluminum ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum ferrosilicon alloy is 20-35 kg / ton, the silicon content of the low aluminum ferrosilicon alloy is 75-80%, and the aluminum content of the low aluminum ferrosilicon alloy is less than 0.5%; During the entire AOD refining process, the basicity of the refined slag was controlled at 1.7±0.1; In the steel tapping process, the tapping temperature is controlled at 1625±25°C; (3) pouring the molten steel refined in the AOD furnace into a dolomite ladle, wherein the refractory layer in contact with the molten steel in the dolomite ladle is made of dolomite material; (4) Continuous casting: The molten steel in the dolomite ladle is continuously casted in a continuous casting machine through a tundish, thereby forming austenitic stainless steel. The composition of inclusions in the austenitic stainless steel comprises: MgAl2O4: 8.0-31.0%, CaO: 9.5-38.0%, SiO2: 32.0-66.0%, and the rest are other inevitable oxides, and the sum of the components of MgAl2O4, CaO and SiO2 accounts for 82-95% of the total components of the inclusions; Before the molten steel is put into the tundish, the air in the tundish is exhausted with protective gas, and protective gas is always introduced into the tundish during the entire continuous casting process.

3. The method for preparing austenitic stainless steel with less slag generated during welding pipe making according to claim 2, characterized in that: In step (1), the molten steel is pre-desulfurized by adding lime into the molten steel.

4. The method for preparing austenitic stainless steel with less slag generated during welding pipe making according to claim 2, characterized in that: In step (2), in the reduction process, when low aluminum silicon ferrosilicon alloy is used for deoxidation, the input amount of the low aluminum silicon ferrosilicon alloy is 30 kg / ton, the silicon content of the low aluminum silicon ferrosilicon alloy is 78%, and the aluminum content of the low aluminum silicon ferrosilicon alloy is less than 0.5%.

5. The method for preparing austenitic stainless steel with less slag generated during welding pipe making according to claim 2, characterized in that: In step (2), the basicity of the refined slag is controlled at 1.7 during the entire AOD refining process.

6. The method for preparing austenitic stainless steel with less slag generated during welding pipe making according to claim 2, characterized in that: In step (2), during the steel tapping process, the steel tapping temperature is controlled at 1625°C.

7. The method for preparing austenitic stainless steel with less slag generated during welding pipe making according to claim 2, characterized in that: In step (4), argon is used as the protective gas.

Citation Information

Patent Citations

  • Method for producing high-purity stainless steel

    CN102943148A

  • Method for controlling plastic inclusions of austenitic stainless steel

    CN105567907A

  • Molten steel inclusion reducing device and stainless steel preparation method capable of improving cleanliness

    CN107974531A

  • Smelting method capable of improving purity of silicon deoxidized molten stainless steel and plasticity of inclusions

    CN111733308A

  • Smelting method of high-purity austenitic stainless steel

    CN111910045A