Hydroelectric steel plate and preparation method thereof

Through reasonable proportion of chemical composition and heat treatment technology, a hydropower steel plate with bainite and martensite microstructure was designed, which solved the problem of poor welding performance of high-strength hydropower steel plates, and achieved the high strength and toughness and welding performance of the steel plates. promote.

CN119061320AActive Publication Date: 2024-12-03SHOUGANG GROUP CO LTD

Patent Information

Application Number
CN202411228547.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

It is difficult to improve welding performance on the basis of ensuring the strength and toughness of the core part of the existing 100mm to 150mm high-strength hydropower steel plate.

Method used

Using the reasonable ratio of chemical components C, Si, Mn, P, S, Alt, Cr, Mo, Cu, Ni, V, B and Fe, the microstructure of bainite and martensite is designed and heated , two-stage rolling, tempering and heat treatment processes, etc., to control the yield strength, tensile strength and low-temperature impact work of steel plates.

Benefits of technology

It realizes the ultra-high strength and toughness of the steel plate and the excellent welding performance, while improving the structure and performance uniformity in the thickness direction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061320A_ABST
    Figure CN119061320A_ABST
Patent Text Reader

Abstract

The invention provides a hydroelectric steel plate and a preparation method thereof, and belongs to the field of steel preparation. The thickness of the steel plate ranges from 100 mm to 150 mm, and the steel plate comprises the chemical components of C, Si, Mn, P, S, Alt, Cr, Mo, Cu, Ni, V, B and Fe. Wherein the content of C ranges from 0.04% to 0.09% by mass, the content of Si ranges from 0.05% to 0.25% by mass, the content of Mn ranges from 0.50% to 1.50% by mass, the content of P is smaller than or equal to 0.007% by mass, the content of S is smaller than or equal to 0.003% by mass, the content of Alt ranges from 0.01% to 0.05% by mass, the content of Cr ranges from 0.20% to 0.80% by mass, the content of Mo ranges from 0.20% to 0.70% by mass, the content of Cu ranges from 0.20% to 2.50% by mass, the content of Ni ranges from 1.0% to 5.0% by mass, the content of V ranges from 0.08% to 0.30% by mass, and the content of B is smaller than or equal to 0.0020% by mass. On the basis of ultra-low carbon, by adopting the component design of low phosphorus and low sulfur and adding a proper amount of microalloy elements such as Ni, Cr and Mo, the metallographic structure of the steel plate is bainite phase transformation and martensite, a structure with excellent comprehensive performance is obtained, and the steel plate obtains ultra-high strength and has excellent low-temperature toughness and welding performance; and meanwhile, the structure and performance uniformity of the steel plate, especially a thick steel plate in the thickness direction is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel preparation, and in particular to a steel plate for hydropower and a preparation method thereof. Background Art

[0002] As traditional energy sources become increasingly scarce, the development and utilization of new energy sources has become a global focus. Therefore, hydropower, as a clean, efficient and renewable energy source, has been widely used and promoted in many countries around the world. At the same time, pumped-storage power stations are also the key to converting unstable power sources such as wind power and solar energy into stable power sources. At present, a large number of 600MPa and 800MPa hydropower steel plates are needed in the construction of hydropower stations, especially pumped-storage power stations, which are mainly used to manufacture key core components such as water diversion pressure pipes and bifurcated pipes, volutes, and units of hydropower stations. In the future, the construction of hydropower stations will develop towards higher heads and larger unit capacities, and the strength level of steel plates needs to be further improved. 1000MPa-level steel plates can reduce the amount of steel used in existing structures by 20%, which can greatly reduce the construction volume and construction costs, and is the future development trend of hydropower steel. At the same time, since the construction of hydropower stations requires a large amount of welding construction in the field, the 1000MPa-level steel plates used in the construction of hydropower stations need to have both good toughness and welding performance.

[0003] Chinese patent CN108315541B discloses a GB-Q&T production method for a 1000MPa grade hydropower steel plate not more than 48mm thick, using a 300mm continuous casting billet, two-stage rolling and then offline quenching and tempering treatment, the yield strength of the steel plate is ≥885MPa, the tensile strength is 950-1130MPa, and KV2 is ≥140J; Chinese patent CN108359879B discloses a DQ-T method for a 1000MPa grade hydropower steel plate not more than 60mm thick, using a 320mm continuous casting billet, two-stage controlled rolling and then online quenching + offline reheating Fire, the yield strength of the steel plate is ≥885MPa, the tensile strength is 950-1130MPa, the elongation is ≥15%, KV2 is ≥100J, and the welding cold crack sensitivity Pcm is ≤0.29%; Chinese patent CN108193137B discloses a DQ-Q&T method for a 1000MPa grade hydropower steel plate with a thickness of no more than 80mm, using a 320mm continuous casting billet, two-stage controlled rolling and then offline tempering treatment, the yield strength of the steel plate is ≥885MPa, the tensile strength is 950-1130MPa, the elongation is ≥15%, and KV2 is ≥70J. Chinese patent CN108385034B discloses a LGB-Q&T method for a 1000MPa grade hydropower steel plate with a thickness of no more than 100mm, using 320mm continuous casting billets, two-stage rolling and water cooling after rolling, and then tempering treatment. The yield strength of the steel plate is ≥865MPa, the tensile strength is 930-1110MPa, and KV2 is ≥47J. The tensile strength level of the hydropower steel plates involved in the above four patents all reaches 1000MPa. However, the thickness specifications of the hydropower steel plates involved in the above four patents do not exceed 100mm. At the same time, due to the extremely high requirements of the service environment and construction environment of the hydropower station on the performance uniformity and weldability of the steel plate, it is required to ensure that the strength and toughness of the steel plate at 1 / 4 and the core reach the same level. The hydropower steel plates involved in the above four patents do not mention how to ensure the mechanical properties of the steel plate thickness core and the welding performance of the steel plate, and how to design the organization of the steel plate to meet the special needs of hydropower steel.

[0004] Therefore, how to improve the welding performance while ensuring the core toughness of 100mm to 150mm thick 1000MPa grade high-strength hydropower steel plates is an urgent problem to be solved. Summary of the invention

[0005] The present application provides a hydropower steel plate and a preparation method thereof to solve the technical problem that the existing 100mm to 150mm thick 1000MPa-level high-strength hydropower steel plate is difficult to improve the welding performance while meeting the core toughness.

[0006] In a first aspect, the present application provides a steel plate for hydropower, wherein the thickness of the steel plate is 100 mm to 150 mm, and the chemical composition of the steel plate includes: C, Si, Mn, P, S, Alt, Cr, Mo, Cu, Ni, V, B and Fe; wherein, in terms of mass fraction,

[0007] The C content is 0.04% to 0.09%, the Si content is 0.05% to 0.25%, the Mn content is 0.50% to 1.50%, the P content is ≤0.007%, the S content is ≤0.003%, the Alt content is 0.01% to 0.05%, the Cr content is 0.20% to 0.80%, the Mo content is 0.20% to 0.70%, the Cu content is 0.20% to 2.50%, the Ni content is 1.0% to 5.0%, the V content is 0.08% to 0.30%, and the B content is ≤0.0020%.

[0008] Optionally, the chemical composition satisfies the following relationship:

[0009] [C]+[Si] / 30+[Mn] / 20+[Cu] / 20+[Ni] / 60+[Cr] / 20+[Mo] / 15+[V] / 10+5[B]≤0.33%,

[0010] In the formula, [C] represents the mass fraction of C, [Si] represents the mass fraction of Si, [Mn] represents the mass fraction of Mn, [Cu] represents the mass fraction of Cu, [Ni] represents the mass fraction of Ni, [Cr] represents the mass fraction of Cr, [Mo] represents the mass fraction of Mo, [V] represents the mass fraction of V, and [B] represents the mass fraction of B.

[0011] Optionally, the microstructure of the steel plate includes bainite and martensite; wherein the volume fraction of the bainite is 15% to 35%, the volume fraction of the martensite is 65% to 85%, the lath width of the bainite and martensite is ≤800nm, and the lath bundle size of the bainite and martensite is <5μm.

[0012] Optionally, precipitated phase particles are dispersed in the matrix structure of the steel plate, the precipitated phase particles include composite carbides of V and Ti and Cu precipitated particles, and the size of the precipitated phase particles is ≤50nm.

[0013] Optionally, the steel plate at the 1 / 4 thickness position and the 1 / 2 thickness position meets at least one of the following properties: yield strength ≥ 850 MPa, tensile strength ≥ 950 MPa, elongation ≥ 15%, and -60°C impact energy KV2 ≥ 80 J.

[0014] In a second aspect, the present application provides a method for preparing a hydropower steel plate according to any one embodiment of the first aspect, the method comprising:

[0015] Obtaining a casting billet having the chemical composition;

[0016] The ingot is heated, rolled in two stages and cooled to obtain a hot-rolled plate;

[0017] The hot rolled plate is subjected to tempering heat treatment to obtain a steel plate for hydropower.

[0018] Optionally, the tempering heat treatment includes heating, quenching, tempering and cooling; wherein, the heating temperature is 840℃~880℃, the heating holding time is 250min~375min, the quenching termination temperature is ≤100℃, the tempering temperature is 620℃~640℃, the tempering holding time is 300min~450min, and air cooling is used for the cooling.

[0019] Optionally, the quenching rate and the temperature of the hot-rolled plate after heating satisfy the following relationship:

[0020] If the temperature of the hot-rolled plate after heating is greater than 500°C, the quenching rate is 0.5°C / s to 15°C / s;

[0021] If the temperature of the hot-rolled plate after heating is 100°C to 500°C, the quenching rate is 0.05°C / s to 5.0°C / s; and,

[0022] The quenching method and the thickness of the hot-rolled plate satisfy the following relationship:

[0023] If the thickness of the hot-rolled plate is 100 mm to 120 mm, a roller quenching machine is used for quenching;

[0024] If the thickness of the hot-rolled plate is greater than 120 mm, a quenching tank is used for the quenching.

[0025] Optionally, the heating temperature is 1100℃~1200℃, and the heating holding time is ≥30min; and / or, the two-stage rolling includes rough rolling and finishing rolling, the rough rolling adopts a large reduction method, the starting rolling temperature of the finishing rolling is 850℃~900℃, the final rolling temperature of the finishing rolling is 760℃~840℃, and the cumulative reduction rate of the finishing rolling is 40%~70%.

[0026] Optionally, the start temperature of the cooling is 730°C to 810°C, the final temperature of the cooling is 100°C to 350°C, and the cooling rate is 5°C / s to 30°C / s.

[0027] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0028] The present application provides a steel plate for hydropower, which realizes the metallographic structure of the steel plate as bainite phase transformation and martensite by adopting low phosphorus and low sulfur and adding appropriate amounts of micro-alloying elements such as Ni, Cr, Mo, etc. on the basis of ultra-low carbon, so as to obtain a structure with excellent comprehensive performance, so that the steel plate obtains ultra-high strength and has excellent low-temperature toughness and welding performance, and at the same time improves the uniformity of the structure and performance of the steel plate, especially the thick-gauge steel plate, in the thickness direction. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0031] Figure 1 A schematic flow chart of a method for preparing a hydropower steel plate provided in an embodiment of the present application;

[0032] Figure 2 The microstructure diagram of the hydropower steel plate provided in Example 1 of the present application;

[0033] Figure 3 The microstructure diagram of the hydropower steel plate provided in Example 2 of the present application;

[0034] Figure 4 The microstructure diagram of the hydropower steel plate provided in Example 3 of the present application;

[0035] Figure 5 This is the microstructure diagram of the hydropower steel plate provided in Example 4 of the present application. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0037] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0038] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.

[0039] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0040] In the first aspect, the present application provides a steel plate for hydropower, the thickness of the steel plate is 100 mm to 150 mm, and the chemical composition of the steel plate includes: C, Si, Mn, P, S, Alt, Cr, Mo, Cu, Ni, V, B and Fe; wherein, in terms of mass fraction, the content of C is 0.04% to 0.09%, the content of Si is 0.05% to 0.25%, the content of Mn is 0.50% to 1.50%, the content of P is ≤0.007%, the content of S is ≤0.003%, the content of Alt is 0.01% to 0.05%, the content of Cr is 0.20% to 0.80%, the content of Mo is 0.20% to 0.70%, the content of Cu is 0.20% to 2.50%, the content of Ni is 1.0% to 5.0%, the content of V is 0.08% to 0.30%, and the content of B is ≤0.0020%.

[0041] The positive effect of controlling the C content to 0.04% to 0.09% is that C is a basic element to ensure the strength and hardness of steel. At the same time, the fine carbides formed with Nb, Ti, etc. can play a role in fine grain and precipitation strengthening, further improving strength and toughness. If the C content is too low, the strength and hardness cannot be guaranteed, and if it is too high, its toughness and weldability will be reduced. For example, the C content can be 0.04%, 0.05%, 0.07%, 0.09%, etc.

[0042] The positive effect of controlling the Si content to 0.05% to 0.25% is that silicon dissolves in ferrite and austenite to improve the hardness and strength of steel. Silicon can shift the C curve to the right and improve the hardenability of steel. However, too high a Si content will deteriorate the plasticity and toughness of steel. For example, the Si content can be 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, etc.

[0043] The positive effects of controlling the Mn content to 0.50% to 1.50% are as follows: Mn can improve the hardness and strength of ferrite and austenite; it can stabilize the austenite structure well and enhance the hardenability of steel; it forms MnS with a higher melting point with sulfur, improving hot working properties and reducing the cold brittle tendency of steel. However, too high a Mn content will cause segregation. Therefore, the added manganese content is controlled to be 0.50% to 1.50%. Exemplarily, the Mn content can be 0.50%, 0.80%, 1.0%, 1.20%, 1.50%, etc.

[0044] The positive effects of controlling the P content ≤ 0.007% and the S content ≤ 0.003% are: P is a harmful element in steel, and its content must be strictly controlled. Phosphorus segregates between grains during the solidification process of steel, causing abnormal local structure of the steel, reducing the grain boundary fracture stress, reducing the plasticity and toughness of the steel, and increasing the ductile-brittle transition temperature, causing cold brittleness, which will damage the welding performance of the steel. The P content should be ≤ 0.007%. For example, the P content can be 0.002%, 0.004%, 0.006%, 0.007%, etc.

[0045] Positive effects of controlling the S content ≤ 0.003%: S is a harmful element in steel, and its content must be strictly controlled. Sulfur can form a low-melting-point FeS eutectic in steel, resulting in hot brittleness. Sulfur can also form sulfides with some other elements, which are distributed in strips along the rolling direction to form a banded structure, which reduces the plasticity and toughness of the steel. The S content should be ≤ 0.003%. Exemplarily, the S content can be 0.001%, 0.002%, 0.003%, etc.

[0046] The positive effect of controlling the content of Alt to 0.01% to 0.05% is that Al has a deoxidizing effect in steel, and adding a small amount of aluminum can refine the grains, thereby improving the strength and impact toughness of the steel. However, if the aluminum content is too high, it will affect the hot working properties, welding properties and cutting properties of the steel. Therefore, the content of Alt is controlled to be 0.01% to 0.05%. For example, the content of Alt can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, etc.

[0047] The positive effect of controlling the Cr content to 0.20% to 0.80% is that Cr increases the hardenability of steel and refines the distance between martensite sheets, thereby increasing the strength of steel and improving the low-temperature impact toughness of steel. However, as the Cr content increases, welding cold cracks are easily generated during welding, which damages the welding performance of steel. The Cr content is controlled to be 0.20% to 0.80%. Exemplarily, the Cr content can be 0.20%, 0.30%, 0.50%, 0.70%, 0.80%, etc.

[0048] The positive effects of controlling the Mo content to 0.20% to 0.70% are: Mo can improve the hardenability of steel, reduce the structural heterogeneity of the steel plate in the thickness direction, improve the strength and improve the low-temperature toughness. In quenched and tempered steel, molybdenum can improve the tempering stability of steel, obtain fine-grained tempered troostite, and improve strength and toughness. However, the cost of Mo alloy is high, so the Mo content is controlled at 0.20% to 0.70%. Exemplarily, the Mo content can be 0.20%, 0.30%, 0.50%, 0.70%, etc.

[0049] The positive effect of controlling the Cu content to 0.20% to 2.50% is that copper precipitates ε-Cu during the tempering process of quenched and tempered steel, producing precipitation strengthening, but if the copper content is too high, the toughness and welding performance of the steel will decrease. Therefore, the Cu content is 0.20% to 2.50%. Exemplarily, the Cu content can be 0.20%, 0.8%, 1.0%, 1.5%, 2.0%, 2.50%, etc.

[0050] The positive effects of controlling the Ni content to 1.0% to 5.0% are: Ni can reduce the austenite transformation temperature, expand the austenite phase region, promote the formation of martensite in the steel, increase the phase difference between martensite and ferrite, increase the resistance of cracks passing through martensite, and improve the low-temperature impact toughness of the steel. However, Ni is expensive, and considering the comprehensive consideration, the Ni content of the steel is controlled at 1.0% to 5.0%. Exemplarily, the Ni content can be 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, etc.

[0051] Positive effects of controlling the V content to 0.08% to 0.30%: V has a strong precipitation strengthening effect, and the content is 0.08% to 0.30%. For example, the V content can be 0.08%, 0.12%, 0.18%, 0.24%, 0.30%, etc.

[0052] The positive effect of controlling the content of B ≤ 0.0020% is that adding an appropriate amount of boron can significantly improve the hardenability of steel, but adding too much boron will affect the toughness and welding performance of steel. Therefore, the content of B should be ≤ 0.0020%. For example, the content of B is 0.0005%, 0.0010%, 0.0015%, 0.0020%, etc.

[0053] In some embodiments, the chemical composition satisfies the following relationship: [C] + [Si] / 30 + [Mn] / 20 + [Cu] / 20 + [Ni] / 60 + [Cr] / 20 + [Mo] / 15 + [V] / 10 + 5 [B] ≤ 0.33%,

[0054] In the formula, [C] represents the mass fraction of C, [Si] represents the mass fraction of Si, [Mn] represents the mass fraction of Mn, [Cu] represents the mass fraction of Cu, [Ni] represents the mass fraction of Ni, [Cr] represents the mass fraction of Cr, [Mo] represents the mass fraction of Mo, [V] represents the mass fraction of V, and [B] represents the mass fraction of B.

[0055] The positive effect of controlling [C]+[Si] / 30+[Mn] / 20+[Cu] / 20+[Ni] / 60+[Cr] / 20+[Mo] / 15+[V] / 10+5[B]≤0.33% is as follows: The cold crack sensitivity index is generally used to judge the welding performance of the steel plate. The larger the value, the worse the weldability. According to the application scenario of the patented steel plate, the steel plate must have good welding performance. Therefore, the cold crack sensitivity index is ≤0.33% to achieve excellent weldability. Exemplarily, the value of the relationship can be 0.10%, 0.15%, 0.20%, 0.25%, 0.33%, etc.

[0056] In some embodiments, the microstructure of the steel plate includes bainite and martensite; wherein the volume fraction of the bainite is 15% to 35%, the volume fraction of the martensite is 65% to 85%, the lath width of the bainite and martensite is ≤800nm, and the lath bundle size of the bainite and martensite is <5μm.

[0057] In some embodiments, precipitated phase particles are dispersed in the matrix structure of the steel plate, the precipitated phase particles include composite carbides of V and Ti and Cu precipitated particles, and the size of the precipitated phase particles is ≤50 nm.

[0058] The microstructure of the steel plate is an ultra-fine martensite structure divided by tempered bainite. After heat treatment, the microstructure of the steel plate at 1 / 4 of the thickness and the core is: tempered ultra-low carbon bainite (accounting for 15% to 35%) + tempered ultra-low carbon martensite (accounting for 65% to 85%); the original austenite grain size of the steel is 10μm to 50μm, among which austenite larger than 30μm will be divided into several regions by low-carbon bainite needles, and each region forms an ultra-low carbon martensite structure, with a lath width of ≤800nm ​​and a lath bundle size of <5μm; there are also dispersed precipitate phase particles in the matrix structure, one is a composite carbide containing V and Ti, and the other is Cu precipitate particles, both of which are within 50nm in size. Exemplarily, the volume fraction of bainite can be 15%, 20%, 25%, 30%, 35%, etc.; the volume fraction of martensite can be 65%, 70%, 75%, 80%, 85%, etc.; the lath width of bainite and martensite can be 500nm, 600nm, 700nm, 800nm, etc.; the lath bundle size of bainite and martensite can be 3μm, 3.5μm, 4μm, etc.; the size of the precipitated phase particles can be 30nm, 35nm, 40nm, 45nm, 50nm, etc.

[0059] In some embodiments, the steel plate at the 1 / 4 thickness position and the 1 / 2 thickness position meets at least one of the following properties: yield strength ≥ 850 MPa, tensile strength ≥ 950 MPa, elongation ≥ 15%, and -60°C impact energy KV2 ≥ 80 J.

[0060] In some embodiments, when the welding heat input is 15 kJ / cm to 30 kJ / cm, the tensile strength of the weld joint is ≥950 MPa, and the impact toughness of the heat-affected zone and the fusion line satisfies the -40°C impact energy KV2 ≥47 J.

[0061] The hydropower steel plate obtained in the present application has both ultra-high strength and toughness and excellent welding performance.

[0062] In a second aspect, the present application provides a method for preparing a hydropower steel plate according to any one of the embodiments of the first aspect, see Figure 1 , the method comprising:

[0063] S1, obtaining a casting billet having the chemical composition;

[0064] In some embodiments, the above step S1 may also include: molten iron desulfurization, converter, LF refining, VD vacuum and continuous casting.

[0065] S2, heating, two-stage rolling and cooling the ingot to obtain a hot-rolled plate;

[0066] In some embodiments, the heating temperature is 1100°C to 1200°C, the total time in the furnace is 380min to 450min, and the heating holding time is ≥30min;

[0067] The comprehensive consideration of heating temperature, furnace time and holding time ensures that the steel billet has the minimum deformation resistance, austenite structure of suitable size, and sufficient dissolution of various micro-alloying elements, so as to exert the best solid solution effect. If the temperature is too high and the time is too long, defects such as overheating, overburning, decarburization, etc. will occur, which will deteriorate the steel plate. It will also make the austenite structure abnormally coarse and unable to be fully refined in the subsequent rolling process, affecting the homogenization and refinement of the structure, which is not conducive to the plastic toughness of the steel plate. The trial steel plate is added with micro-alloying elements such as Nb, Ni, Cr, and Cu. The heating temperature and holding time should ensure that the carbonitride is dissolved as much as possible. If the temperature is too low and the holding time is insufficient, the dissolution amount cannot be guaranteed. If the temperature is too high and the holding time is too long, the structure will be coarse and the effect of refining austenite cannot be achieved. Taking the above factors and production efficiency into consideration, the heating temperature of the steel plate is controlled at 1100℃~1200℃, the heating holding time is ≥30min, and the total furnace time is 380min~450min. Exemplarily, the heating temperature may be 1100° C., 1130° C., 1160° C., 1180° C., 1200° C., etc. Exemplarily, the total furnace time may be 380 min, 400 min, 420 min, 440 min, 450 min, etc. Exemplarily, the heating holding time may be 30 min, 40 min, 50 min, 60 min, 100 min, etc.

[0068] In some embodiments, the two-stage rolling includes rough rolling and finish rolling, the rough rolling adopts a large reduction method, the reduction rate between passes of the rough rolling increases, and the reduction amount of the rough rolling is ≤50 mm.

[0069] The rough rolling stage adopts a large reduction method to enhance the deformation penetration effect in the thickness direction and ensure that the deformation can penetrate into the core. For example, the reduction amount of the rough rolling can be 10mm, 20mm, 30mm, 40mm, 50mm, etc.

[0070] In some embodiments, the start rolling temperature of the finishing rolling is 850° C. to 900° C., the final rolling temperature of the finishing rolling is 760° C. to 840° C., and the cumulative reduction ratio of the finishing rolling is 40% to 70%.

[0071] The steel plate adopts a two-stage rolling process, namely, rolling in the austenite recrystallization zone and rolling in the austenite non-recrystallization zone. The finishing rolling stage mainly adopts the non-recrystallization zone rolling. The finishing rolling start temperature should be 50℃-100℃ lower than the recrystallization temperature. If it is higher than this temperature, it is easy to carry out two-phase rolling, resulting in mixed crystal structure, and this structure is not easy to eliminate in the subsequent rolling process, thereby affecting the plastic toughness. If the finishing rolling start temperature is too low, the metal deformation resistance will increase, which will reduce the deformation amount of a single pass, which is not conducive to the deformation penetration in the thickness direction, and the number of passes needs to be increased to reduce the final rolling temperature. The setting of the final rolling temperature also comprehensively considers the rolling effect and cooling intensity. If the final rolling temperature is too low, the start cooling temperature will be too low, reducing the cooling intensity and rate. The accumulated deformation in the finishing rolling stage is mainly to provide more nucleation sites and retain more dense deformation defects (dislocations, grain boundaries, etc.) during the phase transformation of the deformed supercooled austenite in the subsequent cooling process, so as to make the steel structure more uniform and fine, while improving its strength and toughness. Taking the above factors into consideration, the start rolling temperature of the finishing rolling is controlled to be 850°C to 900°C, the final rolling temperature is 760°C to 840°C, and the cumulative reduction rate is 40% to 70%. For example, the start rolling temperature can be 850°C, 860°C, 870°C, 890°C, 900°C, etc. For example, the final rolling temperature can be 760°C, 780°C, 800°C, 820°C, 840°C, etc. For example, the cumulative reduction rate of the finishing rolling can be 40%, 50%, 60%, 70%, etc.

[0072] In some embodiments, the cooling is performed by water cooling, the start temperature of the cooling is 730°C to 810°C, the end temperature of the cooling is 100°C to 350°C, the cooling rate is 5°C / s to 30°C / s, and air cooling to room temperature is performed after the water cooling is completed.

[0073] Controlled cooling is an important part of the steel plate production process, among which the start cooling temperature, final cooling temperature and cooling rate are important parameters, and their settings are related to the target structure control of the steel plate. If the start cooling temperature is too high, it is related to the final rolling temperature, so that the rolling deformation is restored, and the nucleation position and deformation defects are reduced; if the start cooling temperature is too low, the steel plate enters the transformation zone, and a pre-precipitation structure with low strength is produced, which is not conducive to strength control. The final cooling temperature is related to the phase transformation termination temperature. If the termination temperature is higher than the phase transformation point, the bainite transformation of the steel cannot occur. If it is too low, it will affect the production efficiency. The cooling rate is an important parameter in the controlled cooling of medium and thick plates. At the same time, the setting of the start cooling temperature and the final cooling temperature is more comprehensive. Different cooling rates will cause different phase transformation processes, obtain different phase transformation structures, and affect the grain size, which will ultimately affect the product performance. Uneven cooling rates in the thickness direction of the steel plate will cause uneven distribution of product structure composition and grain size, affecting the product performance. In severe cases, it will also cause plate shape problems due to uneven distribution of stress and strain. Taking the above factors into consideration, the cooling start temperature is controlled to be 730°C to 810°C, the final cooling temperature is 100°C to 350°C, and the cooling rate is 5°C / s to 30°C / s. Exemplarily, the start cooling temperature may be 730°C, 750°C, 780°C, 810°C, etc. Exemplarily, the final cooling temperature may be 100°C, 150°C, 200°C, 300°C, 350°C, etc. Exemplarily, the cooling rate may be 5°C / s, 10°C / s, 15°C / s, 20°C / s, 30°C / s, etc.

[0074] S3. Performing tempering heat treatment on the hot-rolled plate to obtain a steel plate for hydropower.

[0075] In some embodiments, the tempering heat treatment includes heating, quenching, tempering and cooling; wherein the heating temperature is 840°C to 880°C, the heating holding time is 250min to 375min, the quenching termination temperature is ≤100°C, the tempering temperature is 620°C to 640°C, the tempering holding time is 300min to 450min, and air cooling is used for the cooling.

[0076] The steel plate is subjected to a quenching and tempering treatment, including heating, quenching, tempering and cooling processes. The measured phase transition point is 790-830°C, so the heating temperature is set to about 50°C above the phase transition point, and the holding time must ensure sufficient austenite. If it is too low, it cannot be fully austenitized, and if it is too high, the austenitized structure will be too coarse, making the martensite structure coarse after quenching. The quenching termination temperature is the low-temperature martensitic transformation end temperature, and for the sake of production efficiency, it is set to less than 100°C. The tempering temperature is mainly to allow the carbonitrides of the added microalloying elements to be effectively precipitated, and the coarsening is less. If the temperature is too high and the holding time is too long, the carbonitrides will easily coarsen, the strengthening effect will be poor, and the ability to prevent crack propagation will be poor. Taking the above factors into consideration, the quenching heating temperature in the quenching and tempering process is controlled to be 840℃~880℃, the holding time is 250min~375min, the end temperature of quenching is ≤100℃, the temperature of tempering is 620℃~640℃, and the holding time is 300min~450min. Exemplarily, the heating temperature can be 840℃, 850℃, 870℃, 880℃, etc. Exemplarily, the holding time of heating can be 250min, 275min, 300min, 350min, 375min, etc. Exemplarily, the end temperature of quenching can be 50℃, 60℃, 80℃, 100℃, etc. Exemplarily, the temperature of tempering can be 620℃, 625℃, 630℃, 635℃, 640℃, etc. Exemplarily, the holding time of tempering can be 300min, 350min, 400min, 450min, etc.

[0077] In some embodiments, the quenching rate and the temperature of the heated hot-rolled plate satisfy the following relationship:

[0078] If the temperature of the hot-rolled plate after heating is greater than 500°C, the quenching rate is 0.5°C / s to 15°C / s;

[0079] If the temperature of the hot-rolled plate after heating is 100°C to 500°C, the quenching rate is 0.05°C / s to 5.0°C / s; and,

[0080] The quenching method and the thickness of the hot-rolled plate satisfy the following relationship:

[0081] If the thickness of the hot-rolled plate is 100 mm to 120 mm, a roller quenching machine is used for quenching;

[0082] If the thickness of the hot-rolled plate is greater than 120 mm, a quenching tank is used for the quenching.

[0083] Based on ultra-low carbon, targeted composition and hardenability design of steel plates of different thickness specifications are implemented, combined with the control of quenching cooling path during heat treatment process, to achieve step-by-step control of bainite phase transformation and martensite phase transformation, and obtain a structure with excellent comprehensive performance, so that the steel plate can obtain ultra-high strength and excellent low-temperature toughness and welding performance, while improving the uniformity of structure and performance of steel plates, especially thick-specification steel plates, in the thickness direction. Exemplarily, when the temperature of the hot-rolled plate after heating is 500°C, 600°C, 700°C, 800°C, 850°C, etc., the quenching rate may be 0.5°C / s, 2.0°C / s, 5.0°C / s, 10°C / s, 15°C / s, etc.; when the temperature of the hot-rolled plate after heating is 100°C, 200°C, 300°C, 400°C, 500°C, etc., the quenching rate may be 0.05°C / s, 0.5°C / s, 2.0°C / s, 3.0°C / s, 4.0°C / s, 5.0°C / s, etc.; when the thickness of the hot-rolled plate is 100mm, 110mm, 115mm, 120mm, etc., a roller quenching machine is used for the quenching; when the thickness of the hot-rolled plate is 121mm, 130mm, 140mm, 150mm, etc., a quenching pool is used for the quenching.

[0084] The preparation method of the hydropower steel plate is based on the chemical composition of the above-mentioned hydropower steel plate. The specific chemical composition of the hydropower steel plate can be referred to the above-mentioned embodiment. Since the preparation method of the hydropower steel plate adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0085] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0086] Example 1

[0087] Example 1 provides a method for preparing a 100 mm steel plate for hydropower, comprising the following steps:

[0088] Smelting and continuous casting are carried out according to the predetermined composition to obtain a continuous casting billet with a thickness of 400 mm. The chemical composition weight percentage of the continuous casting billet is: C: 0.06%, Si: 0.23%, Mn: 1.02%, P: 0.0043%, S: 0.0011%, Alt: 0.041%, Cr: 0.3%, Mo: 0.35%, Cu: 0.8%, Ni: 2.0%, V: 0.15%, and the remainder is Fe, Pcm=0.25.

[0089] Controlled rolling and controlled cooling process: heating temperature is 1180, total furnace time is 400min, soaking time is 32min. Rough rolling start temperature is 1132℃, rough rolling final rolling temperature is 1080℃, finishing rolling start temperature is 850℃, final rolling temperature is 790℃, start cooling temperature is 754℃, final cooling temperature is 200℃, cooling rate is 25℃ / s, followed by air cooling.

[0090] Offline quenching and tempering heat treatment process: quenching heating temperature 880℃, heating time 250min, quenching using a roller quenching machine, one-time direct cooling, direct cooling to below 100℃, average cooling rate 15℃ / s. Tempering heating temperature 640℃, heating time 300min, cooling method air cooling.

[0091] The transverse mechanical properties of the steel plate described in this example at 1 / 4 of the thickness are as follows: yield strength 910 MPa, tensile strength 989 MPa, elongation 19%, and impact energy KV2 at -60°C is 201 J; the transverse mechanical properties at 1 / 2 of the thickness are as follows: yield strength 899 MPa, tensile strength 967 MPa, elongation 17.5%, and impact energy KV2 at -60°C is 179 J.

[0092] When the heat input of the steel plate welding in this example is 20-23 kJ / cm, the tensile strength at 1 / 4 of the thickness direction of the weld joint is 951 MPa, the impact energy KV2 of the heat affected zone at -40°C is 149 J, and the impact energy KV2 of the fusion line at -40°C is 165 J; the tensile strength at 1 / 2 of the thickness direction of the weld joint is 955 MPa, the impact energy KV2 of the heat affected zone at -40°C is 154 J, and the impact energy KV2 of the fusion line at -40°C is 165 J.

[0093] Example 2

[0094] Example 2 provides a method for preparing a 120 mm steel plate for hydropower, comprising the following steps:

[0095] Smelting and continuous casting are carried out according to the predetermined composition to obtain a continuous casting billet with a thickness of 400 mm. The chemical composition weight percentage of the continuous casting billet is: C: 0.07%, Si: 0.25%, Mn: 0.81%, P: 0.0036%, S: 0.0008%, Alt: 0.034%, Cr: 0.5%, Mo: 0.45%, Cu: 1.2%, Ni: 2.4%, V: 0.22%, and the remainder is Fe, Pcm=0.30.

[0096] Controlled rolling and controlled cooling process: heating temperature is 1180, total furnace time is 402min, soaking time is 30min. Rough rolling start temperature is 1135℃, rough rolling final rolling temperature is 1083℃, finishing rolling start temperature is 900℃, final rolling temperature is 810℃, start cooling temperature is 789℃, final cooling temperature is 200℃, cooling rate is 22℃ / s, followed by air cooling.

[0097] Offline quenching and tempering heat treatment process: quenching heating temperature 860℃, heating time 300min, using roller quenching machine for quenching, by controlling the roller speed and nozzle, using two direct cooling, the first final cooling temperature is 510℃, the cooling rate is 12℃ / s, the second cooling is directly cooled to below 100℃, the average cooling rate is 5℃ / s. Tempering heating temperature 640℃, heating time is 360min, cooling method is air cooling.

[0098] The transverse mechanical properties of the steel plate described in this example at 1 / 4 of the thickness are: yield strength 892 MPa, tensile strength 985 MPa, elongation 19%, and impact energy KV2 at -60°C is 199 J; the transverse mechanical properties at 1 / 2 of the thickness are: yield strength 877 MPa, tensile strength 979 MPa, elongation 18%, and impact energy KV2 at -60°C is 183 J.

[0099] When the heat input of the steel plate welding in this example is 24-29 kJ / cm, the tensile strength at 1 / 4 of the thickness direction of the weld joint is 958 MPa, the KV2 of the heat affected zone at -40°C impact energy is 135 J, and the KV2 of the fusion line at -40°C impact energy is 137 J; the tensile strength at 1 / 2 of the thickness direction of the weld joint is 956 MPa, the KV2 of the heat affected zone at -40°C impact energy is 142 J, and the KV2 of the fusion line at -40°C impact energy is 112 J.

[0100] Example 3

[0101] Example 3 provides a method for preparing a 130 mm steel plate for hydropower, comprising the following steps:

[0102] Smelting and continuous casting are carried out according to the predetermined composition to obtain a continuous casting billet with a thickness of 400 mm. The chemical composition of the continuous casting billet is as follows by weight: C: 0.09%, Si: 0.23%, Mn: 0.77%, P: 0.006%, S: 0.0007%, Alt: 0.025%, Cr: 0.7%, Mo: 0.35%, Cu: 0.97%, Ni: 2.2%, V: 0.25%, and the remainder is Fe, Pcm=0.31.

[0103] Controlled rolling and controlled cooling process: heating temperature is 1210, total furnace time is 425min, soaking time is 40min. Rough rolling start temperature is 1155℃, rough rolling final rolling temperature is 1100℃, finishing rolling start temperature is 900℃, final rolling temperature is 835℃, start cooling temperature is 805℃, final cooling temperature is 302℃, cooling rate is 15℃ / s, followed by air cooling.

[0104] Offline quenching and tempering heat treatment process: quenching heating temperature 850℃, heating time 325min, quenching in a quenching pool, steel plate immersion and air cooling, two direct quenching cooling, the first final cooling temperature is 520℃, cooling rate is 10℃ / s, the second cooling is directly cooled to below 100℃, the average cooling rate is 5℃ / s. Tempering heating temperature 630℃, heating time is 390min, cooling method is air cooling.

[0105] The transverse mechanical properties of the steel plate described in this example at 1 / 4 of the thickness are as follows: yield strength 902 MPa, tensile strength 977 MPa, elongation 18.5%, and impact energy KV2 at -60°C is 204 J; the transverse mechanical properties at 1 / 2 of the thickness are as follows: yield strength 897 MPa, tensile strength 963 MPa, elongation 17.5%, and impact energy KV2 at -60°C is 186 J.

[0106] When the heat input of the steel plate welding in this example is 15-25 kJ / cm, the tensile strength at 1 / 4 of the thickness direction of the weld joint is 947 MPa, the impact energy KV2 of the heat affected zone at -40°C is 138 J, and the impact energy KV2 of the fusion line at -40°C is 85 J; the tensile strength at 1 / 2 of the thickness direction of the weld joint is 958 MPa, the impact energy KV2 of the heat affected zone at -40°C is 149 J, and the impact energy KV2 of the fusion line at -40°C is 89 J.

[0107] Example 4

[0108] Example 4 provides a method for preparing a 150 mm steel plate for hydropower, comprising the following steps:

[0109] Smelting and continuous casting are carried out according to the predetermined composition to obtain a continuous casting billet with a thickness of 400 mm. The chemical composition weight percentage of the continuous casting billet is: C: 0.09%, Si: 0.23%, Mn: 0.75%, P: 0.0033%, S: 0.0009%, Alt: 0.037%, Cr: 0.51%, Mo: 0.35%, Cu: 1.01%, Ni: 3.80%, V: 0.28%, and the remainder is Fe, Pcm=0.33.

[0110] Controlled rolling and controlled cooling process: heating temperature is 1210, total furnace time is 425min, soaking time is 40min. Rough rolling start temperature is 1153℃, rough rolling final rolling temperature is 1100℃, finishing rolling start temperature is 898℃, final rolling temperature is 840℃, start cooling temperature is 810℃, final cooling temperature is 323℃, cooling rate is 12℃ / s, followed by air cooling.

[0111] Offline quenching and tempering heat treatment process: quenching heating temperature 850℃, heating time 375min, quenching in a quenching pool, steel plate immersion and air cooling, two direct quenching cooling, the first final cooling temperature is 520℃, cooling rate is 10℃ / s, the second cooling directly cools to below 100℃, the average cooling rate is 5℃ / s. Tempering heating temperature 630℃, heating time is 450min, cooling method is air cooling.

[0112] The transverse mechanical properties of the steel plate described in this example at 1 / 4 of the thickness are: yield strength 872 MPa, tensile strength 944 MPa, elongation 18.5%, and impact energy KV2 at -60°C is 167 J; the transverse mechanical properties at 1 / 2 of the thickness are: yield strength 855 MPa, tensile strength 931 MPa, elongation 18.5%, and impact energy KV2 at -60°C is 151 J.

[0113] When the heat input of the steel plate welding in this example is 10-18 kJ / cm, the tensile strength at 1 / 4 of the thickness direction of the weld joint is 941 MPa, the impact energy KV2 of the heat affected zone at -40°C is 137 J, and the impact energy KV2 of the fusion line at -40°C is 110 J; the tensile strength at 1 / 2 of the thickness direction of the weld joint is 958 MPa, the impact energy KV2 of the heat affected zone at -40°C is 149 J, and the impact energy KV2 of the fusion line at -40°C is 131 J.

[0114] Attached Figure 2-5 Detailed explanation:

[0115] Depend on Figure 2 It can be seen that the microstructure of the steel plate obtained in Example 1 is tempered martensite (82%) + bainite (16%).

[0116] Depend on Figure 3 It can be seen that the microstructure of the steel plate obtained in Example 2 is tempered martensite (78%) + bainite (20%).

[0117] Depend on Figure 4 It can be seen that the microstructure of the steel plate obtained in Example 3 is tempered martensite (73%) + bainite (24%).

[0118] Depend on Figure 5 It can be seen that the microstructure of the steel plate obtained in Example 4 is tempered martensite (66%) + bainite (31%).

[0119] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0120] (1) In the embodiment of the present invention, a composition design of low carbon, low phosphorus and low sulfur and addition of appropriate amounts of microalloying elements such as Ni, Cr and Mo is adopted, and an offline quenching process with controlled cooling rate is adopted, so that the microstructure at 1 / 4 of the thickness of the steel plate and the core is tempered ultra-low carbon bainite (accounting for 15-35%) + tempered ultra-low carbon martensite (accounting for 65-85%), thereby solving the problem of ensuring the toughness of the core of 1000MPa high-strength hydropower steel plates, especially thick-gauge steel plates, and making the steel plates have excellent welding performance.

[0121] (2) In the embodiments of the present invention, on the basis of ultra-low carbon, targeted composition and hardenability design of steel plates of different thickness specifications are implemented, and the control of the quenching cooling path during the heat treatment process is combined to achieve step-by-step control of the bainite phase transformation and the martensite phase transformation, thereby obtaining a structure with excellent comprehensive performance, so that the steel plate obtains ultra-high strength and has excellent low-temperature toughness and welding performance, and at the same time improves the uniformity of the structure and performance of the steel plate, especially the thick-specification steel plate, in the thickness direction.

[0122] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A steel plate for hydropower, characterized in that: The thickness of the steel plate is 100 mm to 150 mm, and the chemical composition of the steel plate includes: C, Si, Mn, P, S, Alt, Cr, Mo, Cu, Ni, V, B and Fe; wherein, in terms of mass fraction, The C content is 0.04% to 0.09%, the Si content is 0.05% to 0.25%, the Mn content is 0.50% to 1.50%, the P content is ≤0.007%, the S content is ≤0.003%, the Alt content is 0.01% to 0.05%, the Cr content is 0.20% to 0.80%, the Mo content is 0.20% to 0.70%, the Cu content is 0.20% to 2.50%, the Ni content is 1.0% to 5.0%, the V content is 0.08% to 0.30%, and the B content is ≤0.0020%.

2. The steel plate according to claim 1, characterized in that: The chemical composition satisfies the following relationship: [C]+[Si] / 30+[Mn] / 20+[Cu] / 20+[Ni] / 60+[Cr] / 20+[Mo] / 15+[V] / 10+5[B]≤0.33%, In the formula, [C] represents the mass fraction of C, [Si] represents the mass fraction of Si, [Mn] represents the mass fraction of Mn, [Cu] represents the mass fraction of Cu, [Ni] represents the mass fraction of Ni, [Cr] represents the mass fraction of Cr, [Mo] represents the mass fraction of Mo, [V] represents the mass fraction of V, and [B] represents the mass fraction of B.

3. The steel plate according to claim 1, characterized in that: The microstructure of the steel plate includes bainite and martensite; wherein the volume fraction of the bainite is 15% to 35%, the volume fraction of the martensite is 65% to 85%, the lath width of the bainite and martensite is ≤800nm, and the lath bundle size of the bainite and martensite is <5μm.

4. The steel plate according to claim 1, characterized in that: Precipitation phase particles are dispersed in the matrix structure of the steel plate, the precipitation phase particles include composite carbides of V and Ti and Cu precipitation particles, and the size of the precipitation phase particles is ≤50nm.

5. The steel plate according to claim 1, characterized in that: The steel plate at the 1 / 4 position and the 1 / 2 position of the thickness meets at least one of the following properties: yield strength ≥850MPa, tensile strength ≥950MPa, elongation ≥15%, and -60°C impact energy KV2 ≥80J.

6. A method for preparing a steel plate for hydropower use according to any one of claims 1 to 5, characterized in that: The method comprises: Obtaining a casting billet having the chemical composition; The ingot is heated, rolled in two stages and cooled to obtain a hot-rolled plate; The hot rolled plate is subjected to tempering heat treatment to obtain a steel plate for hydropower.

7. The method according to claim 6, characterized in that The tempering heat treatment includes heating, quenching, tempering and cooling; wherein the heating temperature is 840°C to 880°C, the heating holding time is 250min to 375min, the quenching termination temperature is ≤100°C, the tempering temperature is 620°C to 640°C, the tempering holding time is 300min to 450min, and air cooling is used for the cooling.

8. The method according to claim 7, characterized in that The quenching rate and the temperature of the hot-rolled plate after heating satisfy the following relationship: If the temperature of the hot-rolled plate after heating is greater than 500°C, the quenching rate is 0.5°C / s to 15°C / s; If the temperature of the hot-rolled plate after heating is 100°C to 500°C, the quenching rate is 0.05°C / s to 5.0°C / s; and, The quenching method and the thickness of the hot-rolled plate satisfy the following relationship: If the thickness of the hot-rolled plate is 100 mm to 120 mm, a roller quenching machine is used for quenching; If the thickness of the hot-rolled plate is greater than 120 mm, a quenching tank is used for the quenching.

9. The method according to claim 6, characterized in that The heating temperature is 1100°C to 1200°C, and the heating holding time is ≥30min; and / or the two-stage rolling includes rough rolling and finish rolling, the rough rolling adopts a large reduction method, the start rolling temperature of the finish rolling is 850°C to 900°C, the final rolling temperature of the finish rolling is 760°C to 840°C, and the cumulative reduction rate of the finish rolling is 40% to 70%.

10. The method according to claim 6, characterized in that The start temperature of the cooling is 730°C to 810°C, the final temperature of the cooling is 100°C to 350°C, and the cooling rate is 5°C / s to 30°C / s.

Citation Information

Patent Citations

  • A DQ-Q&T method for 1000MPa grade hydroelectric steel plates with a thickness not exceeding 80mm.

    CN108193137B

  • GB-Q&T Production Method for 1000MPa Grade Hydropower Steel Plate with a Thickness Not Greater Than 48mm

    CN108315541B

  • A DQ-T method for 1000MPa grade hydroelectric steel plates with a thickness not exceeding 60mm.

    CN108359879B

  • LGB-Q&T method for 1000MPa grade hydroelectric steel plates with a thickness not exceeding 100mm

    CN108385034B

  • Weldable super-strength steel with excellent low-temperature flexibility and method for manufacturing the same

    CN101676430A

Cited By

  • Large-strain-resistant hydroelectric steel plate with tensile strength of 1000 MPa and preparation method

    CN119843166A

  • A large-strain-resistant hydroelectric steel plate with a tensile strength of 1000 MPa and a preparation method thereof

    CN119843166B