Strong-fatigue-load-resistant ultrahigh-strength steel and heat treatment method thereof

The ultra-high strength steel alloy and heat treatment process enhances the strength and toughness of the steel, achieving a martensitic matrix with improved fatigue resistance and fracture toughness, suitable for aerospace components.

CN119061323AInactive Publication Date: 2024-12-03CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD

Patent Information

Application Number
CN202411423688.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing ultra-high strength steels used in aerospace components, such as 300M steel and Aermet100, have tensile strengths below 2000MPa and fracture toughness limitations, failing to meet the demands of larger civil aircraft and higher load requirements, particularly in landing gear systems.

Method used

A steel alloy composition comprising C, Si, Mn, Cr, Mo, Ni, Co, and fine-grained elements like V and Nb, combined with a heat treatment process involving quenching, cryogenic, and tempering treatments, to achieve a martensitic matrix with enhanced strength-toughness properties.

Benefits of technology

The developed ultra-high strength steel achieves a tensile strength of ≥2200MPa, yield strength of ≥1750MPa, elongation of ≥8%, fracture toughness of ≥60MPa·m 1/2, and a fatigue life of 3 million cycles without failure, addressing the limitations of existing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of ultrahigh-strength steel, in particular to high-fatigue-load-resistant ultrahigh-strength steel and a heat treatment method thereof. A high-toughness martensite matrix is obtained through cooperation of Ni and Co, the tempering resistance of the material is improved through Si and Mn, the ultrahigh-strength steel with excellent strength-toughness matching is obtained, the tensile strength of the ultrahigh-strength steel is larger than or equal to 2200 MPa, the yield strength is larger than or equal to 1750 MPa, the ductility is larger than or equal to 8%, the percentage reduction of area is larger than or equal to 30%, the fracture toughness is larger than or equal to 60 MPa.m < 1 / 2 >, and the yield ratio is larger than or equal to 0.78. The ultrahigh-strength steel provided by the invention has excellent fatigue performance, R is equal to 0.1, Kt is equal to 1, sigma max is equal to 1350 MPa, and the ultrahigh-strength steel is not fractured after the actual measurement fatigue life is 3 million times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of ultra-high strength steel, and in particular to an ultra-high strength steel resistant to strong fatigue loads and a heat treatment method thereof. Background Art

[0002] Due to its ultra-high strength, excellent toughness and fatigue resistance, ultra-high strength steel is widely used in important load-bearing components in the aerospace field, such as aircraft landing gear, engine power shafts, etc.

[0003] The existing main landing gear materials 300M steel and Aermet100 steel have a tensile strength lower than 2000MPa. Higher strength grades such as Aermet310 and Aermet340 have not been put into practical use due to their low fracture toughness. The engineering allowable fatigue load of existing materials is below 1100MPa, which can hardly meet the development trend of larger civil aircraft and higher load on landing gear systems in the future.

[0004] Therefore, it is particularly important to develop an ultra-high strength steel with excellent resistance to high stress fatigue. Summary of the invention

[0005] The present application provides an ultra-high strength steel resistant to strong fatigue loads and a heat treatment method thereof.

[0006] In response to the problem that the strength grade of the existing landing gear trunk material cannot meet the requirements of future large passenger aircraft development, this application develops an ultra-high strength steel resistant to strong fatigue loads and a heat treatment method thereof.

[0007] The present invention obtains a high-toughness martensitic matrix by combining Ni and Co, and uses Si and Mn to improve the tempering resistance of the material, thereby obtaining an ultra-high-strength steel with excellent strength-toughness matching, with a tensile strength of ≥2200MPa, a yield strength of ≥1750MPa, an elongation of ≥8%, a cross-sectional shrinkage of ≥30%, and a fracture toughness of ≥60MPa·m 1 / 2 , yield strength ratio ≥0.78.

[0008] The ultra-high strength steel provided in this application has excellent fatigue performance, R = 0.1, Kt = 1, σ max =1350MPa, the measured fatigue life is 3 million times without breakage.

[0009] In a first aspect, the present application provides an ultra-high strength steel resistant to strong fatigue loads, which adopts the following technical solution:

[0010] The invention discloses an ultra-high strength steel resistant to strong fatigue loads. The chemical composition of the ultra-high strength steel comprises, by mass percentage, C: 0.45-0.55%, Si: 0.5-2%, Mn: 0.2-1.5%, Cr: 0.5-2%, Mo: 0.3-1.5%, Ni: 1-11%, Co: 1-9%, and the balance is Fe and unavoidable impurities.

[0011] Optionally, the ultra-high strength steel contains fine-grained elements, and in terms of mass percentage, the fine-grained elements include V: 0.01-0.2%, and Nb: 0.01-0.10%.

[0012] Optionally, the ultra-high strength steel has a tensile strength of ≥2200 MPa, a yield strength of ≥1750 MPa, an elongation of ≥8%, a cross-sectional shrinkage of ≥30%, and a fracture toughness of ≥60 MPa·m 1 / 2 .

[0013] Optionally, the yield strength ratio of the ultra-high strength steel is ≥0.78.

[0014] Optionally, the ultra-high strength steel has excellent fatigue performance, R = 0.1, Kt = 1, σ max =1350MPa, fatigue life ≥155000 times.

[0015] In a second aspect, the present application provides a heat treatment method for ultra-high strength steel resistant to strong fatigue loads, which adopts the following technical solution:

[0016] A heat treatment method for ultra-high strength steel resistant to strong fatigue loads, the heat treatment method specifically comprising: subjecting an ultra-high strength steel sample that meets chemical composition requirements to quenching treatment, deep cooling treatment, and tempering treatment in sequence.

[0017] Optionally, the quenching treatment includes heating the rod to 870-930° C., keeping the temperature for 0.5-3 hours, and oil cooling.

[0018] Optionally, the cryogenic treatment includes keeping the rod at -196 to 0°C for 0.5 to 4 hours and air cooling it to room temperature.

[0019] Optionally, the tempering treatment includes heating the rod to 160-260° C., keeping the temperature for 1-6 hours, and air cooling to room temperature.

[0020] In summary, the present application includes at least one of the following beneficial technical effects:

[0021] The present invention obtains a high-toughness martensitic matrix by combining Ni and Co, and uses Si and Mn to improve the tempering resistance of the material, thereby obtaining an ultra-high-strength steel with excellent strength-toughness matching, with a tensile strength of ≥2200MPa, a yield strength of ≥1750MPa, an elongation of ≥8%, a cross-sectional shrinkage of ≥30%, and a fracture toughness of ≥60MPa·m 1 / 2 , yield strength ratio ≥0.78.

[0022] The ultra-high strength steel provided in this application has excellent fatigue performance, R = 0.1, Kt = 1, σ max =1350MPa, the measured fatigue life is 3 million times without breakage. DETAILED DESCRIPTION

[0023] Before describing the embodiments of the present application in detail, it should be understood that the terms used herein are only used for the purpose of describing specific embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by ordinary technicians in the field to which the terms belong.

[0024] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of this application, unless otherwise specified, the meaning of "plurality" is two or more.

[0025] The endpoints and any values ​​of the ranges disclosed in this application are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0026] In the present application, the terms "comprise" or "include" are open expressions, that is, including the contents specified in the present application but not excluding other contents.

[0027] The present application provides an ultra-high strength steel resistant to strong fatigue loads, whose chemical composition, in mass percentage, includes C: 0.45-0.55%, Si: 0.5-2%, Mn: 0.2-1.5%, Cr: 0.5-2%, Mo: 0.3-1.5%, Ni: 1-11%, Co: 1-9%, V: 0.01-0.2%, Nb: 0.01-0.10%, and the remainder is Fe and unavoidable impurities.

[0028] The following is a detailed description of the functions and dosage of the components contained in this application:

[0029] Calculated by mass percentage, the ultra-high strength steel of the present application includes C: 0.45-0.55%.

[0030] In the present application, C is the most important strengthening element in low alloy martensitic steel and can play a significant solid solution strengthening effect. Controlling the C content above 0.45% is the key to ensuring its strength. However, the higher the C content, the worse the toughness and plasticity of the material. Therefore, the C content is controlled to be 0.45-0.55%.

[0031] Calculated in percentage by mass, the ultra-high strength steel of the present application includes Si: 0.5-2%, and Mn: 0.2-1.5%.

[0032] In this application, Si can inhibit the decomposition and transformation of retained austenite to Fe3C, improve the tempering resistance of martensite, and significantly increase the tempering temperature, but high Si will reduce the decarburization performance; Mn can improve the hardenability and strength of steel, but too high Mn content will sharply reduce the Ms point, resulting in excessive retained austenite content. Reasonable combination of Si and Mn can enable steel to obtain excellent strength and toughness matching at a suitable tempering temperature, therefore, the Si content is controlled at 0.5-2% and the Mn content is controlled at 0.2-1.5%.

[0033] Calculated by mass percentage, the ultra-high strength steel of the present application includes Cr: 0.5-2%, and Mo: 0.3-1.5%.

[0034] In the present application, Cr can improve the strength of steel through solid solution strengthening and precipitation strengthening, and improve the hardenability and tempering resistance of steel. However, too high Cr content will significantly reduce the Ms of steel, resulting in excessive residual austenite. At the same time, Cr-containing carbides with too high precipitation temperature are likely to exist before solid solution treatment, thereby increasing the solid solution temperature and causing coarse grains and structures; Mo can improve the strength of steel, improve hardenability and tempering resistance, and inhibit the effect of tempering brittleness. However, too high Mo content will increase the quenching temperature, so the Cr content is controlled at 0.5-2% and the Mo content is controlled at 0.3-1.5%.

[0035] Calculated by mass percentage, the ultra-high strength steel of the present application includes Ni: 1-11%, and Co: 1-9%.

[0036] In the present application, Ni can significantly improve the cleavage fracture resistance of the martensitic matrix, but too high a Ni content will form too much residual austenite, which will damage the toughness of the steel and significantly reduce the yield strength of the material; Co can play a role in solid solution strengthening, and inhibit dislocation recovery during tempering, improve tempering resistance, and too high a Co content will damage the toughness of the material. In the present application, the reasonable combination of Ni and Co is the key to obtaining a high-toughness, cleavage-resistant martensitic matrix, therefore, the Ni content is controlled to be 1-11%, and the Co content is 1-9%.

[0037] In terms of mass percentage, the ultra-high strength steel of the present application includes one or more fine-grained elements such as V and Nb, with a V content of 0.01-0.2% and a Nb content of 0.01-0.1%. The carbides and nitrides formed by these elements can effectively inhibit the growth of grains during quenching and heat preservation.

[0038] The ultra-high strength steel provided in the present application also includes inevitable impurity elements, mainly including S, P, O, N, Al, Ti, etc., S≤0.003%, P≤0.005%, O≤0.002%, N≤0.003%, Al≤0.05%, Ti≤0.01%. Effective control of the above impurity elements can improve the toughness and fatigue life of the material.

[0039] The present application also provides a heat treatment method for the ultra-high strength steel, which specifically includes: subjecting an ultra-high strength steel sample that meets the chemical composition requirements to quenching treatment, cryogenic treatment, and tempering treatment in sequence.

[0040] The quenching treatment includes heating the rod to 870-930°C (preferably 900-930°C), keeping the temperature for 0.5-3h, and oil cooling.

[0041] The purpose of quenching is to make the main elements in the steel exist in the matrix in a solid solution state and obtain a martensitic structure during the oil cooling process. If the quenching and holding temperature is too low or the holding time is too short, the alloy elements cannot be fully dissolved. If the quenching and holding temperature is too high or the holding time is too long, it will lead to coarse grains.

[0042] The above-mentioned cryogenic treatment includes cryogenically treating the rod in the range of -196 to 0°C (preferably -40 to 0°C), keeping the temperature for 0.5 to 4 hours (preferably 1 to 2 hours), and air cooling to room temperature.

[0043] Cryogenic treatment is to promote the transformation of retained austenite formed during quenching to martensite.

[0044] The tempering treatment step comprises heating the rod to 160-260° C. (preferably 200-260° C.), keeping the temperature for 1-6 hours (preferably 1-3 hours), and air cooling to room temperature.

[0045] The purpose of tempering treatment is to reduce the hardness of quenched martensite and obtain the matrix structure of tempered martensite and nano-ε carbide, so as to obtain excellent strength and toughness combination.

[0046] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. The embodiments described below are exemplary and are only used to explain the present application, and cannot be interpreted as limiting the present application.

[0047] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0048] The present application is further described in detail below in conjunction with the embodiments and test results.

[0049] Example 1

[0050] This embodiment provides an ultra-high strength steel that is resistant to strong fatigue loads.

[0051] The chemical composition of the above ultra-high strength steel is shown in Table 1 in terms of mass percentage.

[0052] The heat treatment method of the ultra-high strength steel specifically comprises the following steps:

[0053] (1) Quenching treatment: The ultra-high strength steel bars meeting the chemical composition requirements are heated to 900°C, kept at this temperature for 1 hour, and then oil-cooled.

[0054] (2) Cryogenic treatment: The treated bars are cryogenically treated at -73°C, kept warm for 2 h, and then air-cooled to room temperature.

[0055] (3) Tempering treatment: Heat the bar to 240℃, keep it warm for 2h, and air cool it to room temperature.

[0056] Example 2-3

[0057] Embodiments 2-3 respectively provide an ultra-high strength steel resistant to strong fatigue loads.

[0058] The above embodiment is different from embodiment 1 in that the chemical composition of the ultra-high strength steel and the parameter control of the heat treatment process are specifically shown in Table 1 and Table 2. They are consistent with embodiment 1.

[0059] Table 1 Chemical composition of ultra-high strength steel of Examples and Comparative Examples

[0060]

[0061] Table 2 Parameter control of ultra-high strength steel preparation process of embodiment and comparative example

[0062]

[0063] Comparative Example

[0064] Comparative Examples 1-3

[0065] Comparative Examples 1-3 respectively provide an ultra-high strength steel resistant to strong fatigue loads.

[0066] The difference between the comparative example and Example 1 is that the chemical composition of the ultra-high strength steel and the parameter control of the preparation process are specifically shown in Table 1 and Table 2. They are consistent with Example 1.

[0067] Performance test results

[0068] (I) The following tests were performed on the ultra-high strength steels of the above-mentioned embodiments and comparative examples respectively.

[0069] Among them, tensile strength (Rm / MPa), yield strength (R p0.2 / MPa), elongation (A / %), and area reduction (Z / %) are tested in accordance with GB / T 228.1-2010, and fracture toughness (KIC / MPa·m 1 / 2 ) The detection method for ) refers to GB / T 4161-2007.

[0070] The test results are shown in Table 3.

[0071] Table 3 Strength performance test results of ultra-high strength steel of the embodiment and comparative example

[0072] Serial number Rm / MPa <![CDATA[R p0.2 / MPa]]> A / % Z / % <![CDATA[KIC / MPa·m 1 / 2 ]]> Yield-to-strength ratio Example 1 2217 1752 9.5 37 64.8 0.79 Example 2 2206 1752 11.0 47 66.4 0.79 Example 3 2236 1751 10.5 40 63.3 0.78 Comparative Example 1 2208 1648 11.0 42 67.8 0.75 Comparative Example 2 2201 1613 12.0 45 60.6 0.73 Comparative Example 3 1978 1498 11.0 36.0 73 0.76

[0073] As shown in Table 3, the tensile strength of the ultra-high strength steel provided in this application is ≥2200MPa, the yield strength is ≥1750MPa, the elongation is ≥8%, the cross-sectional shrinkage is ≥30%, and the fracture toughness is ≥60MPa·m 1 / 2 , yield strength ratio ≥0.78.

[0074] (ii) Fatigue performance tests were performed on the ultra-high strength steels of Examples 1-2 and Comparative Example 1, respectively.

[0075] Among them, the detection method of fatigue performance test refers to "GB / T 3075-2021".

[0076] The test results are shown in Table 4.

[0077] Table 4 Fatigue performance test results of ultra-high strength steel of the embodiment and comparative example

[0078]

[0079]

[0080] It can be seen from Table 4 that the ultra-high strength steel provided in the present application has significantly excellent fatigue performance.

[0081] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. An ultra-high strength steel resistant to strong fatigue loads, characterized in that: Measured in mass percentage, the chemical composition of the ultra-high strength steel includes C: 0.45-0.55%, Si: 0.5-2%, Mn: 0.2-1.5%, Cr: 0.5-2%, Mo: 0.3-1.5%, Ni: 1-11%, Co: 1-9%, and the remainder is Fe and unavoidable impurities.

2. The ultra-high strength steel according to claim 1, characterized in that: The ultra-high strength steel contains fine-grained elements, which, in terms of mass percentage, include V: 0.01-0.2% and Nb: 0.01-0.10%.

3. The ultra-high strength steel according to claim 1, characterized in that: The ultra-high strength steel has a tensile strength of ≥2200MPa, a yield strength of ≥1750MPa, an elongation of ≥8%, a cross-sectional shrinkage of ≥30%, and a fracture toughness of ≥60MPa·m 1 / 2 .

4. The ultra-high strength steel according to claim 1, characterized in that: The yield strength ratio of the ultra-high strength steel is ≥0.

78.

5. The ultra-high strength steel according to claim 1, characterized in that: The ultra-high strength steel has excellent fatigue performance, R=0.1, Kt=1, σ max =1350MPa, fatigue life ≥155000 times.

6. A heat treatment method for high fatigue load resistant ultra-high strength steel according to any one of claims 1 to 5, characterized in that: The heat treatment method specifically includes: subjecting an ultra-high strength steel sample that meets the chemical composition requirements to quenching treatment, deep cooling treatment, and tempering treatment in sequence.

7. The heat treatment method according to claim 6, characterized in that: The quenching treatment includes heating the rod to 870-930° C., keeping the temperature for 0.5-3 hours, and oil cooling.

8. The heat treatment method according to claim 6, characterized in that: The cryogenic treatment includes keeping the rod at -196~0°C for 0.5-4h and air cooling to room temperature.

9. The heat treatment method according to claim 6, characterized in that: The tempering treatment includes heating the rod to 160-260° C., keeping the temperature for 1-6 hours, and air cooling to room temperature.

Citation Information

Patent Citations

  • Low-temperature tempered martensite ultrahigh-strength steel

    CN103147020A

  • Fire-resistant steel of ocean platform with excellent anti-fatigue performance and production method thereof

    CN103243261A

  • High-ductility ultrahigh-toughness steel and preparation method thereof

    CN113249645A

  • Martensitic steel with ultrahigh strength and high plasticity and toughness and preparation method thereof

    CN114774800A

  • Economical high-toughness ultrahigh-strength steel and preparation method thereof

    CN116288067A

Cited By

  • High-impact-toughness steel plate with yield strength of 1550 MPa and preparation method of high-impact-toughness steel plate

    CN120400714A