Downhole drilling tool part and manufacturing method and application thereof
By forming a Ni3Al intermetallic compound wear-resistant layer in easily wear-resistant parts of the downhole drilling tool parts, the problems of welding cracks and high costs in traditional wear-resistant alloys are solved, and the effect of improving wear resistance and reducing costs is achieved.
Patent Information
- Application Number
- CN202411167792.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional downhole drilling tool parts have early failure of wear between internal parts, resulting in reduced tool service life, and traditional wear-resistant alloys have welding crack problems and high costs.
The wear-resistant layer of Ni3Al intermetallic compound as the carcass is formed in the easily worn parts of the underground drilling tool parts. Pre-alloy powder of cast chromium carbide and boron elements is prepared by vacuum smelting, and the automatic cladding equipment is used to cladd in the friction area to form resistance. Abrasive layer improves wear resistance and reduces costs.
It improves the wear resistance of downhole drilling tools parts, extends service life, and reduces material and processing costs. The wear resistance of the wear-resistant layer is increased by more than 20%, and avoids the occurrence of welding cracks.
Smart Images

Figure CN119061395A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of wear-resistant technology, in particular to the field of metal parts surface strengthening technology, and to a downhole drilling tool part and a manufacturing method and application thereof. Background Art
[0002] During the oil drilling process, the internal parts of oil drilling tools such as roller drill bits and screw drills wear each other, causing these tools to fail early due to severe wear between parts, reducing the service life of the tools and ultimately causing the tools to be scrapped early.
[0003] Traditional wear-resistant technology mainly solves the wear problem between the internal parts of downhole drilling tools by surfacing wear-resistant alloys on the easily worn parts between the internal parts of downhole drilling tools. These wear-resistant alloys are mainly traditional Stellite alloys and some Fe-based wear-resistant alloys. The former has high hardness and is prone to defects such as welding cracks; the latter has low wear resistance and a greater tendency to weld cracks. The appearance of cracks will inevitably lead to a decrease in wear resistance, thereby causing the early failure of downhole drilling tools. At the same time, traditional Stellite alloys are cobalt-based alloys, and their material and processing costs are both high, which is not economical. Summary of the invention
[0004] The purpose of the present invention is to provide a downhole drill tool part and a manufacturing method thereof, and a downhole drill tool comprising the downhole drill tool part, so as to protect the easily worn parts between the downhole drill tool parts and improve the service life of the downhole drill tool.
[0005] In order to achieve the above-mentioned purpose of the invention, the present invention forms a wear-resistant layer with Ni3Al intermetallic compound as the matrix metal in the area where the downhole drill tool parts are subjected to internal friction of the downhole drill tool, which can improve the service life of the downhole drill tool parts. In addition, the material cost and processing cost of the manufacturing method are low, and the economy is good.
[0006] In a first aspect, the present invention provides a method for manufacturing a downhole drilling tool part, comprising the following steps:
[0007] The Ni3Al intermetallic compound, cast chromium carbide with a particle size of 120 to 400 meshes, and boron element are vacuum melted together, and then atomized to prepare a pre-alloyed powder with a particle size of 100 to 325 meshes; the pre-alloyed powder contains, by weight percentage: C: 1.35wt% to 2.25wt%, Cr: 13.65wt% to 22.75wt%, Al: 9.98wt% to 11.30wt%, B: 0.02wt% to 0.07wt%, and the rest is Ni and unavoidable impurities;
[0008] Preheat the part substrate to 280-350°C;
[0009] Automatic cladding equipment is used to clad the pre-alloyed powder into a wear-resistant layer in the area of the part that is subject to internal friction of the downhole drilling tool.
[0010] In some embodiments provided by the present invention, the weight percentage of the cast chromium carbide in the pre-alloyed powder is 15wt% to 25wt%.
[0011] In some embodiments provided by the present invention, automatic cladding equipment is used to clad the pre-alloyed powder in the area of the part subject to internal friction of the downhole drill tool to form a wear-resistant layer using a PTA cladding process, with a current of 110 to 150A, a voltage of 25 to 30V, a welding speed of 180 to 220mm / min, and a powder feeding speed of 8 to 12g / min.
[0012] In some embodiments provided by the present invention, the part substrate is steel.
[0013] In some embodiments provided by the present invention, Ni3Al intermetallic compound, cast chromium carbide with a particle size of 120 to 400 mesh, and boron element are vacuum melted together, comprising:
[0014] Under vacuum conditions, Ni3Al intermetallic compounds are melted at 1490°C to 1540°C, and cast chromium carbide and boron element with a particle size of 120 to 400 meshes are added and mixed to obtain an alloy melt.
[0015] In some embodiments provided by the present invention, the thickness of the wear-resistant layer is 2 to 3.5 mm.
[0016] In some embodiments provided by the present invention, the automatic cladding equipment is one of plasma cladding (PTA) equipment, laser cladding (LC) equipment, and electron beam cladding (EBC) equipment.
[0017] In some embodiments provided by the present invention, the powder feeding method of the automatic cladding equipment is coaxial powder feeding or side-axis powder feeding.
[0018] In a second aspect, the present invention provides a downhole drilling tool component manufactured by the above-mentioned downhole drilling tool component manufacturing method.
[0019] In some embodiments provided by the present invention, the downhole drilling tool part is a cone bearing of a roller drill bit or a universal shaft of a screw drill.
[0020] In a third aspect, the present invention provides a downhole drilling tool, which includes the downhole drilling tool parts mentioned above.
[0021] Compared with the prior art, the technical solution provided by the present invention has the following advantages and beneficial effects:
[0022] The wear-resistant layer obtained by the manufacturing method of the downhole drilling tool parts provided by the present invention has high stress wear resistance. Compared with the wear-resistant layer prepared by using Stellite 190 alloy under the same method, the wear resistance is improved by more than 20%, and the material cost is also low. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 : Typical microstructure of Ni3Al+chromium carbide in the wear-resistant layer prepared in Example 1 (500X).
[0024] Figure 2 : Typical microstructure of Stellite 190 cobalt-based alloy in the wear-resistant layer prepared in Comparative Example 2 (500X). DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range. Similarly, any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.
[0027] It should be noted that, in the description of this article, unless otherwise specified, "above", "below" are inclusive numbers, and the meaning of "multiple" in "one or more" is two or more. Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.
[0028] In the description of this specification, the description with reference to the terms "any embodiment / method", "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.
[0029] The above summary of the invention of the present invention is not intended to describe each disclosed embodiment or each implementation in the present invention. The following description more specifically illustrates exemplary embodiments. These embodiments can be used in various combinations. In each example, the enumeration is only used as a representative group and should not be interpreted as exhaustive.
[0030] Overlay welding is a process of depositing a layer of metal of the same or different material on the surface of metal parts or metal rolled products by welding. Studies have found that cracks are inevitable in the overlay layer, and these cracks affect the wear resistance of the overlay layer to a certain extent. Due to the high hardness and high stress of the overlay wear-resistant layer, cracks will inevitably expand. In severe cases, various problems such as the overlay layer and the substrate are not firmly bonded and the surface is peeling off will occur. In order to solve such problems, the following measures are generally adopted in this field: select suitable substrates and transition materials; reduce the thickness of the overlay layer, or select impact-resistant overlay materials; adopt preheating, slow cooling, intermediate tempering, and multiple tempering to remove residual stress.
[0031] For the surface strengthening of forgings such as toothed bearings and universal joints with steel bases, the process route of the existing technology is: toothed bearings: surfacing - rough turning - heat treatment - fine turning, the surfacing step uses Stellite alloy, Stellite alloy has high hardness and is prone to welding cracks, which affects wear resistance; universal joints: heat treatment - surfacing - fine milling, the surfacing step uses Fe-based wear-resistant alloy, Iron-based wear-resistant alloy is also prone to welding cracks, which affects wear resistance.
[0032] Manufacturing method
[0033] The invention provides a method for manufacturing a downhole drilling tool part, comprising the following steps: vacuum melting Ni3Al intermetallic compound, cast chromium carbide with a particle size of 120-400 meshes, and boron element, and then preparing pre-alloy powder with a particle size of 100-325 meshes by atomization; the pre-alloy powder comprises, by weight percentage, 1.35wt%-2.25wt% of C, 13.65wt%-22.75wt% of Cr, 9.98wt%-11.30wt% of Al, 0.02wt%-0.07wt% of B, and the rest is Ni and inevitable impurities; preheating a part substrate to 280-350°C; and using automatic cladding equipment to clad the pre-alloy powder in an area of the part subject to internal friction of the downhole drilling tool to form a wear-resistant layer.
[0034] The present invention uses Ni3Al intermetallic compound as matrix metal and cast chromium carbide as wear-resistant phase to make the wear-resistant layer. The Ni3Al intermetallic compound has high heat resistance, thermal conductivity, oxidation resistance and toughness, and can reduce the tendency of crack formation; the cast chromium carbide has high hardness and can be used as a wear-resistant phase and reinforcement phase to improve the tensile strength and wear resistance of the wear-resistant layer.
[0035] In the prior art, Fe-based alloy powder is prepared by gas atomization: the raw materials are placed in a smelting furnace to be melted and alloyed in a short time, and then gas atomized to make powder, and the powder obtained by atomization is screened to obtain Fe-based alloy powder. The Fe-based alloy powder is mechanically mixed with cast tungsten carbide powder to obtain plasma surfacing alloy powder. This surfacing alloy powder is only a mechanical mixture of Fe-based alloy powder and cast tungsten carbide powder. The comparative example of the present invention adopts a similar method to the above-mentioned method to mechanically mix Ni3Al intermetallic compound powder and cast chromium carbide powder evenly, and prepares it into a wear-resistant layer by cladding process. It is found that the wear-resistant layer is segregated. It is speculated that this is because the density of nickel-based alloy powder and cast chromium carbide powder is different, resulting in agglomeration and stratification of the mixed powder. During the cladding process, cast chromium carbide particles settle at the bottom of the wear-resistant layer, which ultimately leads to a low content of cast chromium carbide on the surface of the wear-resistant layer and insufficient wear resistance.
[0036] The present invention pre-forms Ni3Al intermetallic compound particles and cast chromium carbide particles into pre-alloyed powder, and makes the cast chromium carbide particles uniformly dispersed in the Ni3Al intermetallic compound matrix to form Ni3Al intermetallic compound particles covering the cast chromium carbide, and then quickly clads the particles on the surface of the substrate in the cladding stage, so as to avoid the cast chromium carbide particles from settling in the Ni3Al metal melt, thereby preparing a uniform wear-resistant layer.
[0037] The wear-resistant layer obtained by the present invention has the advantages of low density, high strength, good high-temperature mechanical properties and oxidation resistance, and is just suitable for working conditions where downhole drilling tools are heavily loaded and severely worn.
[0038] In the pre-alloyed powder used in the present invention, the weight percentage of cast chromium carbide is 15% to 25%. The weight percentage of cast chromium carbide within the above range can ensure that the wear-resistant layer has high toughness and wear resistance, and has less friction with the mating parts.
[0039] The substrate for manufacturing downhole drilling tool parts of the present invention is 15CrNiMo alloy. The substrate used in the embodiment is forged 15CrNiMo alloy, which has high strength and heat resistance. The present invention prepares a wear-resistant layer with Ni3Al intermetallic compound as the matrix metal in the area where the parts are subjected to internal friction of the downhole drilling tool, which can not only improve the wear resistance of the parts, but also improve their corrosion resistance and impact resistance. The chemical composition of the pre-alloyed powder of the present invention can match the substrate material, and no transition layer is required between the two, that is, it has a high bonding strength, so that the wear-resistant layer is not easy to fall off from the substrate.
[0040] The purpose of preheating the part substrate to 280-350° C. in the present invention is to prevent the cladding liquid formed by melting the pre-alloyed powder from rapidly solidifying when cooled, thereby forming welding defects at the interface between the part substrate and the wear-resistant layer, thereby causing welding cracks.
[0041] Before preheating the part substrate to 280-350° C., the surface of the substrate needs to be cleaned to remove impurities such as oil and rust. The surface cleaning of the substrate includes one or more of washing, sandblasting, and grinding, and its purpose is to reduce the roughness of the substrate surface and avoid the generation of cracks due to the substandard surface roughness of the substrate.
[0042] The present invention vacuum melts Ni3Al intermetallic compound, cast chromium carbide with a particle size of 120 to 400 meshes, and boron element together, including: melting Ni3Al intermetallic compound at 1490°C to 1540°C under vacuum conditions, adding cast chromium carbide with a particle size of 120 to 400 meshes and boron element and mixing them to obtain alloy melt. In this process, Ni3Al intermetallic compound melts, while cast chromium carbide does not melt, and cast chromium carbide has a large density, so the alloy melt needs to be heated and stirred to avoid the cast chromium carbide from settling in the alloy melt; during the spraying process, the alloy melt with evenly dispersed cast chromium carbide is quickly cooled to become pre-alloyed powder.
[0043] When the alloy melt is atomized, the invention uses a fast-moving fluid (atomizing medium) to impact or otherwise break the alloy melt into fine droplets, which are then condensed into alloyed powder. Each particle in the alloyed powder not only has the same uniform chemical composition as the given molten alloy (wear-resistant layer), but also refines the crystal structure due to rapid solidification, eliminating the macroscopic segregation of the second phase.
[0044] Specifically, the process steps of making pre-alloyed powder of the present invention are as follows: first, Ni3Al intermetallic compound is smelted into alloy melt (1490℃~1540℃) in an electric furnace or induction furnace under vacuum environment, then refractory casting chromium carbide (120~400 mesh, melting point is above 1780℃) and boron element (content is 0.02wt%~0.07wt% of the total amount of pre-alloyed powder) are added, and stirred evenly, and injected into a tundish located above the atomizing nozzle. The alloy melt flows out from the leak at the bottom of the tundish, and when passing through the nozzle, it meets the high-speed airflow or water flow and is atomized into fine droplets, and the atomized droplets are quickly solidified into pre-alloyed powder (100~325 mesh) in a closed atomizing tube, and each pre-alloyed powder formed has exactly the same uniform chemical composition-Ni3Al-based chromium carbide pre-alloyed powder.
[0045] In the present invention, the weight percentage of cast chromium carbide in the pre-alloyed powder is 15wt% to 25wt%, which can ensure that the wear resistance of the wear-resistant layer is enhanced without affecting the overall strength of the wear-resistant layer.
[0046] The present invention uses automatic cladding equipment to clad the pre-alloy powder in the area of the part that is subject to internal friction of the downhole drilling tool to form a wear-resistant layer. The parameters are set as follows: the current is 110-150A, the voltage is 25-30V, the welding speed is 180-220mm / min; the powder feeding speed is 8-12g / min. Under this condition, the pre-alloy powder is melted and penetrates each other with the molten iron alloy on the surface of the part substrate to produce a metallurgical reaction. The two solidify at a similar temperature to form a Ni3Al+chromium carbide solid solution structure, avoiding the occurrence of segregation, thereby ensuring that the cladding layer and the substrate are well bonded, and the cladding layer has a uniform structure and is not easy to fall off from the substrate surface.
[0047] The manufacturing method of the present invention controls the thickness of the wear-resistant layer to 2 to 3.5 mm. Under this thickness, it can ensure that the wear-resistant layer is not strong enough due to the high thickness, and can also ensure that the parts have enough wear-resistant layer for wear. The present invention performs lathe processing after surfacing welding on the surface of the gear bearing to form a wear-resistant layer with a thickness of 2.5-3 mm, leaving a 1.5-2 mm thick margin; the present invention performs milling processing after surfacing welding on the surface of the universal shaft to form a wear-resistant layer with a thickness of 5-6 mm, leaving a margin of about 3.5 mm. Since the wear-resistant layer needs to be machined after surfacing welding, the wear-resistant layer of the present invention has a lower hardness and is easier to machine than the wear-resistant layer of the Stellite 190 alloy powder with a higher hardness.
[0048] In addition, the wear-resistant layer in the present invention also needs to have low friction with the mating parts to ensure the service life of the mating parts. The wear-resistant layer of the present invention using Ni3Al intermetallic compound as the matrix metal has a ceramic-like surface with low roughness and high hardness, thereby ensuring that the wear-resistant layer itself has high wear resistance while having low friction with the mating parts.
[0049] In some embodiments provided by the present invention, the automatic cladding equipment is one of plasma cladding (PTA) equipment, laser cladding (LC) equipment, and electron beam cladding (EBC) equipment.
[0050] In some embodiments provided by the present invention, the powder feeding method of the automatic cladding equipment is coaxial powder feeding or side-axis powder feeding.
[0051] Downhole drilling tool parts
[0052] The present invention provides a downhole drilling tool part manufactured by the manufacturing method of the downhole drilling tool part. The wear-resistant layer on the downhole drilling tool part manufactured by the manufacturing method has low hardness, good toughness, and is not easy to crack. Therefore, it has good wear resistance, is not easy to wear, and has a long service life. In some embodiments, the downhole drilling tool part is a tooth palm bearing of a roller drill bit or a universal shaft of a screw drill.
[0053] Downhole drilling tools
[0054] The present invention provides a downhole drilling tool, which includes the downhole drilling tool parts. The wear-resistant layer on the downhole drilling tool parts manufactured by the manufacturing method has low hardness, is not easy to crack, has good wear resistance, is not easy to wear, and has a long service life, thereby ensuring the service life of the downhole drilling tool.
[0055] Example
[0056] The technical scheme of the present invention is described in detail by way of examples below. If the manufacturer's brand or preparation method is not specified, the raw materials, equipment or solvents used are all common raw materials, equipment or solvents on the market. Unless otherwise specified, the raw materials of the same name used in the following examples and comparative examples are all the same raw materials.
[0057] Example 1
[0058] This embodiment provides a method for manufacturing a tooth palm bearing of a roller drill bit, the process flow is: surfacing-rough turning-heat treatment-finishing turning, and the surfacing process includes the following steps:
[0059] 1. First, use an electric furnace or an induction furnace to melt the Ni3Al intermetallic compound into an alloy melt (1500℃) in a vacuum environment, then add refractory cast chromium carbide (120-400 mesh, melting point 1780℃) and boron element (content of 0.05wt% of the total amount of pre-alloyed powder) to increase toughness, stir evenly, and inject it into the tundish located above the atomizing nozzle. The alloy melt flows out from the leak at the bottom of the tundish, and when passing through the nozzle, it encounters a high-speed airflow or water flow and is atomized into fine droplets. The atomized droplets are quickly solidified into pre-alloyed powder (100-325 mesh) in a closed atomizing tube. Each pre-alloyed powder formed has exactly the same uniform chemical composition. The composition of the pre-alloyed powder is: Cr: 16wt%, Al: 11wt%, C: 1.6wt%, B: 0.05wt%, and the rest is Ni and unavoidable impurities.
[0060] 2. Clean, sandblast or polish the surface of the forged 15CrNiMo alloy toothed bearing substrate to remove impurities such as oil, rust, etc., and preheat to 350℃.
[0061] 3. Put the prepared pre-alloyed powder into the automatic PTA cladding equipment, and clad the surface of the area of the tooth palm bearing that is subjected to the internal friction of the downhole drill by coaxial powder feeding to form a 3.0mm thick wear-resistant layer. Cladding parameters: workpiece preheating temperature: 350℃; shielding gas: argon (purity ≥99.99%), flow rate 12L / min; plasma gas: argon, flow rate 1.35L / min; powder feeding gas: argon, flow rate 2.5L / min; welding parameters: current: 130A, voltage: 28V, welding speed: 200mm / min; powder feeding speed: 10g / min.
[0062] After rough turning and before heat treatment, the hardness and microstructure of the cladding layer were tested. The hardness of the wear-resistant layer was HRC38-42. The microstructure diagram is as follows: Figure 1 shown.
[0063] Example 2
[0064] This embodiment provides a method for manufacturing a universal shaft of an ultra-high torque screw drill, the process flow of which is: heat treatment - surfacing - fine milling, and the surfacing process includes the following steps:
[0065] 1. First, use an electric furnace or an induction furnace to melt the Ni3Al intermetallic compound into an alloy melt (1500℃) under a vacuum environment, then add refractory cast chromium carbide (120-400 mesh, melting point 1780℃) and boron element (content is 0.05wt% of the total amount of pre-alloyed powder) to increase toughness, stir evenly, and inject it into the tundish located above the atomizing nozzle. The alloy melt flows out from the leak at the bottom of the tundish, and when passing through the nozzle, it encounters a high-speed airflow or water flow and is atomized into fine droplets. The atomized droplets are quickly solidified into pre-alloyed powder (100-325 mesh) in a closed atomizing tube. Each pre-alloyed powder formed has exactly the same uniform chemical composition. The composition of the pre-alloyed powder is: Cr: 20wt%, Al: 10wt%, C: 2wt%, B: 0.05wt%, and the rest is Ni and unavoidable impurities.
[0066] 2. Clean, sandblast or polish the surface of the forged LS3 alloy universal shaft substrate to remove impurities such as oil, rust, etc., and preheat to 350°C.
[0067] 3. Put the prepared pre-alloyed powder into the automatic laser cladding equipment, and form a 2.0mm thick wear-resistant layer in the area of the universal bearing of the ultra-high torque screw drill that is subjected to the internal friction of the downhole drill by coaxial powder feeding. Cladding parameters: workpiece preheating temperature: 350℃; protective gas: argon (purity ≥99.99%), flow rate 30L / min; semiconductor laser, laser power 4000W, scanning speed: 135mm / min; powder feeding speed: 25g / min. Three layers of wear-resistant layer are clad together, and finally milled to the final thickness.
[0068] Comparative Example 1
[0069] This comparative example provides a method for manufacturing a universal shaft of an ultra-high torque screw drill, the process flow of which is: heat treatment-surfacing-fine milling, and the surfacing process includes the following steps:
[0070] 1. Ni3Al powder with a particle size range of 100 to 270 mesh, cast chromium carbide powder, and boron element are mixed together to obtain a cladding material; the chemical composition of the cladding material is: Al: 11.3wt%, C: 1.35wt%, Cr: 13.65wt%, B: 0.05wt%, and the balance is Ni and other trace elements, wherein the weight ratio of cast chromium carbide is about 15wt%.
[0071] 2. Place the cladding material into the automatic laser cladding equipment, and clad the area of the universal bearing of the ultra-high torque screw drill that is subject to internal friction of the downhole drill by coaxial powder feeding to form a 2.0mm thick wear-resistant layer. Cladding parameters: workpiece preheating temperature: 350℃; protective gas: argon (purity ≥99.99%), flow rate 30L / min; semiconductor laser, laser power 4000W, scanning speed: 135mm / min; powder feeding speed: 25g / min. Three layers of wear-resistant layer are clad in total, and finally milled to the final thickness.
[0072] Due to the different densities of the cast chromium carbide powder, Ni3Al powder and ferroalloy powder during the powder mixing and welding process, the powders agglomerate and stratify, resulting in defects such as segregation or cracks in the wear-resistant layer prepared in this comparative example.
[0073] Comparative Example 2
[0074] This comparative example provides a method for manufacturing a tooth palm bearing of a roller drill bit, and the process flow is: surfacing-rough turning-heat treatment-finishing turning, and the surfacing process includes the following steps:
[0075] 1. Put the Stellite 190 alloy powder into the automatic PTA cladding equipment, and clad the area of the palm bearing that bears the internal friction of the downhole drill bit by coaxial powder feeding to form a 3.0mm thick wear-resistant layer. Cladding parameters: workpiece preheating temperature: 350℃; shielding gas: argon (purity ≥99.99%), flow rate 12L / min; plasma gas: argon, flow rate 1.35L / min; powder feeding gas: argon, flow rate 2.5L / min; welding parameters: current: 95A, voltage: 26V, welding speed: 40mm / min; powder feeding speed: 15g / min.
[0076] The Stellite 190 alloy powder used in this comparative example is a high-carbon cobalt-chromium-tungsten alloy powder with a particle size of 100-270 mesh, and its typical composition is: C: 3.4wt%, Cr: 26wt%, W: 14wt%, Ni: <2wt%, Mo: <1wt%, Fe: <2wt%, Si: <1wt%, and the balance is Co and unavoidable impurities.
[0077] After rough turning and before heat treatment, the hardness and microstructure of the cladding layer are tested. The hardness of the wear-resistant layer is HRC55-61. The microstructure diagram is as follows: Figure 2 The wear-resistant layer formed in this comparative example is about 3.5 mm, and due to the high hardness of the wear-resistant layer, crack defects are very likely to occur.
[0078] The wet sand wear test of the metal wheel shows that the wear resistance of the wear-resistant layer of Comparative Example 2 is about 1.35 (1 / g), which is about 35% lower than the wear resistance of the wear-resistant layer of Example 1 of 2.08 (1 / g). It is speculated that this is because the wear-resistant layer of Example 1 has a higher strength, thereby ensuring better wear resistance.
[0079] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but should conform to the widest scope consistent with the principles and novel features invented herein.
Claims
1. A method for manufacturing downhole drilling tool parts, It is characterized in that The following steps are involved: Ni 3 Al intermetallic compound, cast chromium carbide with a particle size of 120 to 400 meshes, and boron element are vacuum melted together, and then atomized to form a pre-alloyed powder with a particle size of 100 to 325 meshes; in terms of weight percentage, the pre-alloyed powder contains: C: 1.35wt% to 2.25wt%, Cr: 13.65wt% to 22.75wt%, Al: 9.98wt% to 11.30wt%, B: 0.02wt% to 0.07wt%, and the rest is Ni and unavoidable impurities; Preheat the part substrate to 280-350°C; Automatic cladding equipment is used to clad the pre-alloyed powder into a wear-resistant layer in the area of the part that is subject to internal friction of the downhole drilling tool.
2. The method for manufacturing downhole drilling tool parts according to claim 1, Features: The weight percentage of the cast chromium carbide in the pre-alloyed powder is 15wt% to 25wt%.
3. The method for manufacturing downhole drilling tool parts according to claim 1, Features: Automatic cladding equipment is used to clad the pre-alloyed powder into a wear-resistant layer in the area of the part subject to internal friction of the downhole drilling tool. The PTA cladding process is adopted with a current of 110-150A, a voltage of 25-30V, a welding speed of 180-220mm / min, and a powder feeding speed of 8-12g / min.
4. The method for manufacturing downhole drilling tool parts according to claim 1, Features: Ni 3 Al intermetallic compound, cast chromium carbide with a particle size of 120 to 400 mesh, and boron element are vacuum melted together, including: Ni under vacuum conditions 3 The Al intermetallic compound is melted at 1490°C to 1540°C, and cast chromium carbide and boron element with a particle size of 120 to 400 meshes are added and mixed to obtain an alloy melt.
5. The method for manufacturing downhole drilling tool parts according to claim 1, Features: The thickness of the wear-resistant layer is 2 to 3.5 mm.
6. The method for manufacturing downhole drilling tool parts according to claim 1, Features: The automatic cladding equipment is one of plasma cladding equipment, laser cladding equipment and electron beam cladding equipment.
7. The method for manufacturing downhole drilling tool parts according to claim 1, Features: The powder feeding method of automatic cladding equipment is coaxial powder feeding or side-axis powder feeding.
8. A downhole drilling tool part, Features: The downhole drilling tool component is manufactured by the manufacturing method of any one of claims 1 to 7.
9. The downhole drilling tool component according to claim 8, Features: The downhole drilling tool parts are the cone bearing of the roller drill bit or the universal shaft of the screw drill.
10. A downhole drilling tool, Features: Including the downhole drilling tool parts according to claim 8 or 9.