Laser cladding alloy powder for die steel surface, preparation method and use method
By using laser cladding alloy powder containing C, W, Cr, Nb, Mn, V, Mo and Ni on the surface of the mold steel to form a high-performance cladding layer, the wear resistance of the cold-working mold steel in the prior art is solved. The problem of this is to realize low-cost and high-performance mold steel materials, extend the service cycle and reduce replacement costs.
Patent Information
- Application Number
- CN202411439233.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art has not yet effectively improved the wear resistance and service life of commonly used cold-working mold steels, and it is difficult to meet the demand for high-temperature performance of automobile lightweight manufacturing at low cost.
A laser cladding alloy powder used for the surface of mold steel is adopted, and the composition includes C, W, Cr, Nb, Mn, V, Mo and Ni. Through specific preparation and use methods, the tensile strength is ≥1800MPa and the yield strength are formed. Laser cladding layer with ≥1100MPa, fracture elongation A≥8%, and room temperature microhardness ≥410HV after heat treatment at 620°C.
It significantly improves the mechanical properties and wear resistance of mold steel, extends the service cycle, is low in cost and excellent in performance, and the service cycle of the mold matrix can be nearly twice as good.
Smart Images

Figure CN119061397A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to tool steel and a production method, and in particular to laser cladding alloy powder for the surface of die steel, a preparation method and a use method. Background Art
[0002] Lightweighting is an important development direction for achieving energy conservation and emission reduction in automobiles. At present, hot stamping and integrated die-casting technologies are widely used in the field of lightweight manufacturing of automobile parts; their molds usually work under high temperature conditions and need to have good red hardness and wear resistance, and hot working die steel is generally used.
[0003] Although hot working die steel (such as H13, 2344, 8407, QRO90, etc.) has good high temperature wear resistance, it has a high alloy content and is expensive. Conventional cold working die steel (such as P20, 9Mn2V, 9SiCr, CrWMn, etc.) has the characteristics of good toughness and low cost; however, due to its low alloy content of Cr, W, Ni, etc., its high temperature wear resistance is insufficient. At present, the automotive lightweight industry urgently needs a low-cost, high temperature resistant die steel material.
[0004] The recently emerged laser cladding technology is expected to become a new solution for material surface modification. Laser cladding uses a high-energy laser beam as an energy source to melt the metal cladding powder layer by layer according to the three-dimensional CAD slice model data to form a high-performance, high-density and high-precision cladding layer. This cladding layer is tightly combined with the substrate and has the characteristics of dense structure and fine grains, which can greatly improve the mechanical properties of the mold. At the same time, by cladding a thin layer of high-performance material on the mold surface, the use of materials is greatly reduced and the cost is reduced. Since the performance of this laser cladding layer mainly depends on the cladding layer material and the cladding process, the research and development of cladding materials and the corresponding additive manufacturing methods have always been valued by researchers.
[0005] After searching:
[0006] The document with Chinese patent publication number CN 112941503 A proposes "A method for improving the hardness of H13 steel", whose components include: C: ≤0.5%, but not 0; Si: 0.5-6%; Mn: 0.01-0.11%; P: 0.01-0.07%; S: 0.01-0.06%; Cr: 6-13%; Mo: ≤1.2%, but not 0; Ti: 0.0-0.6%; V: 1.0-1.8%; the rest is Fe and unavoidable impurities. Its preparation method is: H13 steel is used as the substrate, and the parts of the substrate surface that need to be surfacing are pretreated such as one or more of cleaning, heating, and grinding. One or more layers of high-hardness alloy in powder form are surfacing on the surface of the substrate to prepare the required metal material. The total thickness of the high-hardness alloy layer welded on the surface of the substrate is 5-25mm, and the thickness of each layer of the high-hardness alloy is 0.5-2.5mm. The material layer is irradiated with a laser or electron beam above the material layer, causing at least part of the high-hardness alloy to melt into a molten state, and cooling and forming a solidified layer to form each layer. In the process of cladding the high-hardness alloy on the surface of the substrate by laser cladding, the power of the laser is 1200-1800W, the laser scanning speed is 5-10mm / s, the powder feeding amount is 20-50g / min, and the diameter of the spot formed by the laser is 0.8-1.3mm. The surface of the metal material after cladding is finely processed to form a smooth surface. The Rockwell hardness of the surface cladding strengthening layer is 57-59HRC, which is relatively low; there is no report on its wear resistance.
[0007] The document with Chinese patent publication number CN 112442691 A proposes "A kind of automobile stamping die insert and its laser strengthening manufacturing method", whose components include: C: 0.15~0.17%; Si: ≤0.04%; Cr: 17~19%; Ni: 0.27%; Mo: 0.3%; Mn: ≤0.2%; Co: ≤0.12%; V: ≤0.08%; B: ≤0.27%, and the rest is Fe. The preparation method is as follows: pre-treat the mold insert: remove the surface layer of 1 to 2 mm thick on the surface of the mold insert by mechanical processing, and then perform tempering treatment at 500 to 600 ° C; prepare the cladding layer alloy powder, the alloy powder is spherical particles with a particle size of 50 to 150 μm; place the mold insert on the workbench of the laser cladding equipment for clamping and positioning, coaxially convey the alloy powder, and use the alloy powder to repeatedly laser clad the outer surface of the mold insert. The conditions for laser cladding are: the protective gas flow rate is 10-15L / min, the powder feeder speed is 1.5 to 2.0r / min, the laser power is 1300W, and the scanning speed is 15mm / min. A cladding strengthening layer with a thickness of 1.5 to 2mm is made; the mold insert with the cladding strengthening layer is mechanically processed. The Rockwell hardness of the surface cladding strengthening layer is 58-60HRC, which is relatively low; there is no report on its wear resistance.
[0008] The document with Chinese patent publication number CN 114645200 A proposes "A high-toughness, high-thermal stability die steel and its preparation method", whose components include: C: 0.33%-0.38%; Si: 0.88%-1.12%; Mn: 0.25%-0.45%; S: ≤0.010%; P: ≤0.010%; Cr: 4.85%-5.20%; Mo: 1.10%-1.75%; V: 0.50%-0.60%; Ce: 0.025%-0.038%; Y: 0.082%-0.095%; Ni≤0.10%; Cu≤0.10%; the rest is Fe; the Rockwell hardness of its surface cladding strengthening layer is 46.9-48.8HRC, and no comparison of its wear resistance is seen.
[0009] The document with Chinese patent publication number CN 109881109 A proposes "A laser cladding material and a method for preparing a laser cladding coating", whose components include: C: 0.5%-0.85%; Si: 0.2%-0.5%; Mn: 0.3%-0.4%; Cr: 8%-10%; Mo: 4%-5%; V: 0.3%-0.5%; the balance is Fe. The preparation method comprises the following steps: weighing furnace charge according to the component proportion, melting the furnace charge in a non-vacuum induction furnace, oxidizing and deslagging, and transferring the deslagging to an LF furnace for refining; adding lime and fluorite to the LF furnace, adding ferrosilicon for alloying after slagging and deoxidation stabilization in the LF furnace, feeding Al wire calculated according to Al0.2% into the LF furnace for precipitation deoxidation; heating the ladle refining furnace seat, adjusting the ladle slag system composition, and ensuring that the mass ratio of the sum of CaO and CaF2 in the refining slag to the mass ratio of the slag is 65-70%; transferring the furnace to a VD furnace for vacuum refining, using argon gas with a flow rate of 300-400NL / min for stirring before vacuum treatment, blowing argon at the bottom of the ladle for stirring while maintaining vacuum pressure, The argon flow rate is 150-200NL / min, ensuring that the residual gas H is ≤2.0ppm. After degassing, sampling and analysis are completed. After passing the test, the steel liquid is soft-blown by bottom blowing argon for 15-20min, and the steel ingot is cast by pouring method; the obtained steel ingot is forged, the initial forging temperature is 1120-1140℃, the final forging temperature is 890-910℃, and it is cooled to 250-350℃ to obtain a forged alloy with a forging ratio of 5; the forged alloy is refined and spheroidized annealed to obtain the mold steel body; the mold steel body is modified by laser cladding, and an alloy composite layer is formed on the mold steel body to obtain a mold steel with high toughness and high thermal stability. The Vickers hardness of the surface cladding strengthening layer is 779-819HV (equivalent to 83 to 84HRC), and no comparison of its wear resistance is seen.
[0010] The document with Chinese patent publication number CN 110284136 A proposes a laser remanufacturing method for automobile stamping dies, which includes the following components: C: 0.65-0.75%; Si: 0.85-1.15%; Mn: 0.65-1.05%; P: ≤0.03%; S: ≤0.03%; Cr: 0.90-1.20%; Mo: 0.20-0.50%; V: 0.15-0.30%; the rest is Fe; the preparation method is: pre-treat the overall material of the die to keep it clean as a whole , clean; detect the actual hardness of the mold base material, select the mold with an actual hardness of HRC30-40 for remanufacturing; select powder for the mold according to the working conditions, turn on the agitator of the powder feeder to load powder; open the gas to test the powder, turn on the switch on the nitrogen bottle, adjust the nitrogen delivery volume so that the delivery value is 5mbar, adjust the air pressure gauge detection value of the powder feeder to between 6-8mbar, and start the gas test button; start the powder feeder button to focus the powder, and feed according to the processing height of the mold surface. Powder focusing; turn on the spot of the semiconductor laser, adjust the laser head through the trial teaching device, so that the spots of the powder feeder and the laser head are at the same focus; adjust the gas pressure of the shielding gas, turn on the compressed air filter, use compressed air as the shielding gas, and use a five-stage filtration system for filtration. The inlet of the compressed air is filtered through the second stage, and the outlet is filtered through the third stage. The filtered gas is adjusted by the ball valve instrument. The gas volume is adjusted to 2-5mbar. The ball valve instrument is connected to the laser head through the air pipe to protect the protective lens of the laser head; test parameters, use semiconductor laser to perform selective cladding in the area that does not affect the processing area and the quality of the automobile stamping die itself, adjust the working parameters of the laser cladding according to the test results, and record the working parameters after meeting the working conditions; plan the repair path of laser cladding, and formulate the repair path in combination with the actual object or according to the characteristics of the mold; turn on the gas, water, and laser on site, start the equipment trial operation program, and simulate and confirm the process route; start the equipment normally and perform laser cladding on the mold. The Rockwell hardness of the surface cladding strengthening layer is 50-52HRC, and no comparison of its wear resistance is found.
[0011] In summary, there is no report on surface strengthening based on common cold working die steel to improve its surface hardness and wear resistance so that it can be used in hot stamping, integrated die casting and other industries. Therefore, in order to improve the wear resistance and service life of die steel and reduce costs, it is urgent to develop a low-cost, high-performance laser cladding alloy material and its additive manufacturing method. Summary of the invention
[0012] The present invention aims to overcome the shortcomings of the prior art and provide a laser cladding alloy powder for mold steel surface, a preparation method and a use method thereof, wherein the mechanical properties of the laser cladding layer on the mold surface are as follows: tensile strength ≥1800MPa, yield strength ≥1100MPa, elongation at break A ≥8%, microhardness ≥410HV at room temperature after heat treatment at 620°C, impact energy ≥110J, and a service life that is nearly twice that of the mold substrate.
[0013] Measures to achieve the above objectives:
[0014] A laser cladding alloy powder for the surface of a mold steel, wherein the components and contents of the laser cladding alloy powder are: C: 0.60-0.64wt.%, W: 1.9-2.1wt.%, Cr: 3.9-4.1wt.%, Nb: 0.75-0.85wt.%, Mn: 0.9-1.1wt.%, V: 0.9-1.0wt.%, Mo: 2.4-2.6wt.%, Ni: 0.08-0.12wt.%, and the balance is Fe and unavoidable impurities.
[0015] Preferably, the content of W is 1.95-2.05% by weight.
[0016] Preferably, the content of Nb is 0.75-0.80 wt.%.
[0017] A method for preparing laser cladding alloy powder for mold steel surface, comprising the following steps:
[0018] 1) The raw materials described in claim 1 are proportioned and mixed uniformly, and then conventionally smelted into a melt;
[0019] 2) preparing the cladding powder by atomization, mechanical crushing, reduction, electrolysis or vapor deposition, and sieving the cladding powder with a particle size of 5 to 70 μm after cooling to room temperature with the furnace;
[0020] 3) Dry the cladding powder, control the drying temperature at 75-85°C, and the drying time is not less than 5.5h;
[0021] 4) Allow to cool naturally to room temperature and set aside for later use.
[0022] A method for using laser cladding alloy powder on a mold steel surface, comprising the following steps:
[0023] 1) Screening the cladding powder prepared in claim 2 to screen out cladding powder with a particle size of 5 to 60 μm;
[0024] 2) Add cladding powder with a particle size of 5 to 60 μm into the powder feeding cylinder of the selective laser melter, which is equipped with a scanner;
[0025] 3) Set the working parameters of the selective laser melter: laser power: 180W~200W, laser scanning speed: 790~
[0026] 810mm / s; thickness of each layer of cladding powder: 35-37μm, scanning spacing: 0.075-0.085mm;
[0027] 4) Clean the surface of the mold substrate to be processed, that is, polish and remove rust, clean with alcohol and dry until there is no moisture on the mold surface;
[0028] 5) Preheating the mold substrate at a temperature of 80 to 100°C for 2 to 5 hours;
[0029] 6) Start the selective laser melter, and spread the cladding powder prepared in claim 2 through the powder feeding cylinder for multiple passes, and simultaneously perform laser scanning under the protection of protective gas until the laser cladding alloy powder layer clad on the mold surface reaches a thickness of 2 to 3 mm.
[0030] The laser scans the same layer in the same direction as the laying of the cladding powder; when laying another layer, the scanning is performed at a rotation angle.
[0031] The invention is characterized in that the laser scanner on the selective laser melter and the selective laser melter can be operated separately.
[0032] Functions and mechanisms of the components and main processes in the present invention
[0033] C: Carbon can promote grain refinement. After grain refinement, the alloy not only has higher strength, but also has enhanced toughness. This dual improvement in strength and toughness enables the alloy powder to withstand greater stress and deformation during the manufacturing process, thereby improving the reliability and service life of the product.
[0034] W: Tungsten is a metal with a high melting point and high hardness, which makes it an ideal element to improve the heat resistance and wear resistance of the alloy. Adding tungsten to the alloy powder can significantly improve the stability and wear resistance of the alloy at high temperatures. The addition of tungsten can also enhance the strength and hardness of the alloy. The solid solution strengthening effect of tungsten atoms in the alloy causes the alloy's lattice to distort, thereby improving the strength and hardness of the alloy.
[0035] Mn: Manganese can significantly improve the hardenability of steel, allowing the steel to obtain a deeper hardened layer after quenching. This is very important for steels that require high hardenability, such as spring steel, bearing steel, and tool steel. By improving the hardenability, these steels can have higher hardness and wear resistance after quenching.
[0036] Cr: Chromium can significantly improve the hardness and wear resistance of carbon steel without making the steel brittle. When the Cr content exceeds a certain value, the hardness and wear resistance of the steel will be further improved. This makes the Cr-containing steel have better durability when subjected to wear and friction. The Cr element can also reduce the stacking fault energy of the alloy and significantly improve the high-temperature endurance strength of the alloy. This makes the Cr-containing alloy have better stability and durability in high-temperature environments.
[0037] Nb: Niobium is dissolved in the alloy matrix, which hinders dislocation movement by generating lattice distortion, thereby improving the strength of the alloy; at the same time, it can stabilize the formation of carbides, inhibit intergranular corrosion and intragranular corrosion, thereby improving the corrosion resistance of the alloy. In high-temperature alloys, Nb can improve the creep strength of the alloy, making the alloy have better stability and durability in high-temperature environments.
[0038] V: Vanadium can be used as a grain refiner to refine the grain structure of the alloy by inhibiting the growth of grains. Fine grains can improve the strength and toughness of the alloy, and also help improve the fatigue strength and impact resistance of the alloy. Vanadium can increase the hardenability of steel, allowing the alloy to obtain a deeper hardened layer during the quenching process. This helps to improve the overall strength and hardness of the alloy. Improve red hardness: Vanadium can also significantly improve the hardness and wear resistance of the alloy at high temperatures, that is, red hardness. This allows the alloy to maintain good mechanical properties and wear resistance in high temperature environments.
[0039] Mo: Molybdenum can inhibit the segregation of harmful elements at the grain boundary, thereby reducing the brittleness of the alloy during tempering and improving the toughness and plasticity of the alloy. Mo can delay the transformation of pearlite, but has little effect on the transformation of bainite, thereby improving the hardenability of the alloy, allowing the alloy to obtain a deeper hardened layer after quenching; at the same time, it can also improve the electrical conductivity and thermal conductivity of the alloy, and reduce the expansion coefficient of the alloy.
[0040] Ni: Nickel can be used as an austenite stabilizing element to improve the strength and toughness of the alloy by refining the grains and strengthening the solid solution. Nickel usually exists in the alloy in the form of solid solution, which increases the strength and hardness of the alloy by increasing the bonding force of atoms in the solid solution. At the same time, nickel can also refine pearlite, making the alloy's structure more uniform and further improving the mechanical properties.
[0041] The reason why the present invention controls the drying temperature of the cladding powder to be between 75 and 85°C and the drying time to be not less than 5.5 hours is that the cladding powder may absorb moisture in the air during storage and use. If these moisture are not removed, defects such as pores and inclusions will occur during the cladding process, seriously affecting the quality and performance of the cladding layer. Therefore, the moisture in the powder can be effectively removed by drying to ensure the quality of the cladding layer. At the same time, at high temperatures, the powder is prone to oxidation reactions, resulting in decreased powder performance. Controlling the drying temperature within the range of 75 to 85°C can significantly reduce the risk of powder oxidation. A longer drying time (not less than 5.5 hours) can ensure that the moisture in the powder is fully evaporated, while avoiding excessively high temperatures that cause powder oxidation.
[0042] The reason why the particle size of the laser cladding alloy powder layer is controlled to be 5-60 μm is that when the particle size of the powder is too large, the gaps between the heated powder particles will cause a capillary effect, so that the metal liquid cannot fully fill the gaps, thereby increasing the porosity of the formed part. If the particle size of the powder is too small, the powder particles will melt quickly during the heating process, making it difficult to control the density of the formed part, which will also affect the density of the formed part.
[0043] The reason why the present invention controls the working parameters of the selective laser melter: laser power 180W~200W, laser scanning speed 790~810mm / s; the thickness of each layer of cladding powder is 35~37μm, and the scanning spacing is 0.075~0.085mm, is because the power range of 180W to 200W is usually sufficient to ensure that the powder material is fully melted, while avoiding defects such as spatter and pores caused by excessive melting. Within this power range, the laser melting process is relatively stable and not easily affected by external environmental fluctuations, which is conducive to obtaining consistent cladding quality; the scanning speed determines the residence time of the laser beam on the powder layer, which in turn affects the melting efficiency and the size of the heat-affected zone. Within the speed range of 790 to 810mm / s, appropriate melting depth and width can be obtained, while reducing the range of the heat-affected zone and reducing the risk of deformation and cracking; the thickness of the powder layer directly affects the precision of the formed part and the interlayer bonding strength. The thickness range of 35 to 37 μm is conducive to obtaining good interlayer bonding and fine forming effects, while reducing the generation of defects such as pores and cracks; the scanning spacing determines the degree of overlap between adjacent molten pools, which in turn affects the microstructure and performance of the formed part. The spacing range of 0.075 to 0.085 mm can usually obtain good molten pool overlap and uniform microstructure, which is conducive to improving the strength and toughness of the formed part.
[0044] The reason why the present invention controls the substrate preheating temperature at 80-100°C and the preheating time at 2-5h is that the substrate may generate certain internal stress during processing or storage. By preheating, the stress in the substrate can be released to avoid deformation or cracking in the subsequent process. At the same time, preheating can also improve the fluidity of the solder, which is conducive to the uniform distribution of the solder on the substrate and improves the welding quality; the length of the preheating time directly affects the preheating effect. Too short preheating time may not allow the substrate to reach the required preheating temperature, and too long preheating time may cause the substrate to be over-preheated, thereby increasing the risk of deformation of the substrate. At the same time, excessive preheating may also thicken the oxide film on the surface of the substrate, which is not conducive to the combination between the cladding powder and the substrate, thereby affecting the cladding effect. The appropriate preheating time can ensure that the substrate reaches a stable preheating temperature, providing a good foundation for the subsequent cladding process.
[0045] The reason why the present invention undergoes multiple passes of laser cladding and laser scanning of the same layer under the protection of a protective gas until the laser cladding alloy powder layer clad on the mold surface reaches a thickness of 2 to 3 mm is that a single cladding of too thick a coating may cause the heat-affected zone to be too large, increasing the risk of thermal deformation and cracking of the substrate material. Through multiple passes of cladding, the heat input can be dispersed, and the thermal effect of each cladding on the substrate can be reduced, thereby reducing the possibility of deformation and cracking. Multiple passes of cladding help to improve the organizational structure and performance of the cladding layer. Each cladding layer undergoes a certain heat treatment and phase change process during the solidification process. Through multiple cladding and solidification, the grains can be refined, defects can be reduced, and the hardness and wear resistance of the cladding layer can be improved. The protective gas (such as an inert gas) can effectively isolate the air and prevent the molten pool and the cladding layer from being oxidized, thereby maintaining the chemical composition and performance of the cladding layer.
[0046] Compared with the prior art, the mechanical properties of the laser cladding layer on the mold surface of the present invention are as follows: tensile strength ≥1800MPa, yield strength ≥1100MPa, elongation at break A ≥8%, microhardness ≥410HV at room temperature after heat treatment at 620°C, impact energy ≥110J, and the service life can be nearly twice that of the mold substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The morphology photo of the laser cladding alloy cladding powder of the present invention;
[0048] Figure 2 The microstructure of the junction between the cladding material and the mold substrate of the present invention;
[0049] Figure 3 The microstructure of the cladding material of the present invention;
[0050] Figure 4 It is a line graph showing the hardness of the cladding layer of the present invention changing with laser power. DETAILED DESCRIPTION
[0051] The present invention is described in detail below:
[0052] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;
[0053] Table 2 is a list of main process parameters for preparing laser cladding alloy powders of various embodiments and comparative examples of the present invention;
[0054] Table 3 is a list of main process parameters for the laser cladding alloy powders of various embodiments and comparative examples of the present invention;
[0055] Table 4 is a table of performance test results of various embodiments of the present invention and comparative examples.
[0056] Each embodiment of the present invention is produced according to the following steps
[0057] A method for preparing laser cladding alloy powder for mold steel surface, comprising the following steps:
[0058] 1) The raw materials described in claim 1 are proportioned and mixed uniformly, and then conventionally smelted into a melt;
[0059] 2) preparing the cladding powder by atomization, mechanical crushing, reduction, electrolysis or vapor deposition, and sieving the cladding powder with a particle size of 5 to 70 μm after cooling to room temperature with the furnace;
[0060] 3) Dry the cladding powder, control the drying temperature at 75-85°C, and the drying time is not less than 5.5h;
[0061] 4) Allow to cool naturally to room temperature and set aside for later use.
[0062] A method for using laser cladding alloy powder on a mold steel surface, comprising the following steps:
[0063] 1) Screening the cladding powder prepared according to claim 2 to screen out cladding powder with a particle size of 5 to 60 μm;
[0064] 2) Add cladding powder with a particle size of 5 to 60 μm into the powder feeding cylinder of the selective laser melter, which is equipped with a scanner;
[0065] 3) Setting the working parameters of the selective laser melter: laser power: 180W-200W, laser scanning speed: 790-810mm / s; thickness of each layer of cladding powder: 35-37μm, scanning spacing: 0.075-0.085mm;
[0066] 4) Clean the surface of the mold substrate to be processed, that is, polish and remove rust, clean with alcohol and dry until there is no moisture on the mold surface;
[0067] 5) Preheating the mold substrate at a temperature of 80 to 100°C for 2 to 5 hours;
[0068] 6) Start the selective laser melter, and spread the cladding powder prepared in claim 2 through the powder feeding cylinder for multiple passes, and simultaneously perform laser scanning under the protection of protective gas until the laser cladding alloy powder layer clad on the mold surface reaches a thickness of 2 to 3 mm.
[0069] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0070]
[0071] Table 2 List of main process parameters for preparation and use of laser cladding alloy powders in various embodiments of the present invention and comparative examples
[0072]
[0073]
[0074] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0075]
[0076] It can be seen from Table 3 that there are significant differences in the mechanical properties of the embodiments of the present invention and the comparative examples. By comparing the embodiments, it can be found that the mechanical property parameters such as yield strength and tensile strength of different embodiments are different, among which many properties of embodiment 1 are relatively excellent, indicating that after the composition of the cladding powder is fine-tuned, the mechanical properties of the material will change.
[0077] Compared with the comparative examples, the examples generally show higher values in key mechanical performance parameters such as yield strength and tensile strength, indicating that the material or method provided by the present invention can significantly improve the mechanical properties of the material. Parameters such as elongation, hardness and hardness after heat treatment also show the advantages of the examples over the comparative examples, indicating that the present invention improves the hardness and durability of the material while maintaining its toughness.
[0078] Because the embodiments generally show higher values in mechanical performance parameters such as yield strength and tensile strength. This means that under the same stress conditions, the materials used in the embodiments can withstand greater loads, thereby possibly reducing waste caused by material failure. Therefore, the embodiments improve the utilization rate of materials and reduce costs. At the same time, the present invention can be used to repair damaged molds, extend the service life of the molds, save manpower and material resources consumed in the mold replacement process, and greatly reduce the cost of mold replacement.
[0079] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A laser cladding alloy powder for die steel surface, Features: The components and contents of the laser cladding alloy powder are: C: 0.60-0.64wt.%, W: 1.9-2.1wt.%, Cr: 3.9-4.1wt.%, Nb: 0.75-0.85wt.%, Mn: 0.9-1.1wt.%, V: 0.9-1.0wt.%, Mo: 2.4-2.6wt.%, Ni: 0.08-0.12wt.%, and the balance is Fe and unavoidable impurities.
2. The laser cladding alloy powder for die steel surface according to claim 1, Features: The content of W is 1.95-2.05%wt.%.
3. The laser cladding alloy powder for die steel surface according to claim 1, Features: The content of Nb is 0.75-0.80 wt.%.
4. A method for preparing a laser cladding alloy powder for a mold steel surface as claimed in claim 1, comprising the following steps: 1) The raw materials described in claim 1 are proportioned and mixed uniformly, and then conventionally smelted into a melt; 2) preparing the cladding powder by atomization, mechanical crushing, reduction, electrolysis or vapor deposition, and sieving the cladding powder with a particle size of 5 to 70 μm after cooling to room temperature with the furnace; 3) Dry the cladding powder, control the drying temperature at 75-85°C, and the drying time is not less than 5.5h; 4) Allow to cool naturally to room temperature and set aside for later use.
5. The method for using the laser cladding alloy powder for the surface of mold steel according to claim 1, comprising the steps of: 1) Screening the cladding powder prepared in claim 2 to screen out cladding powder with a particle size of 5 to 60 μm; 2) Add cladding powder with a particle size of 5 to 60 μm into the powder feeding cylinder of the selective laser melter, which is equipped with a scanner; 3) Setting the working parameters of the selective laser melter: laser power: 180-200W, laser scanning speed: 790-810mm / s; thickness of each layer of cladding powder: 35-37μm, scanning spacing: 0.075-0.085mm; 4) Clean the surface of the mold substrate to be processed, that is, polish and remove rust, clean with alcohol and dry until there is no moisture on the mold surface; 5) Preheating the mold substrate at a temperature of 80 to 100°C for 2 to 5 hours; 6) Start the selective laser melter, and spread the cladding powder prepared in claim 2 through the powder feeding cylinder for multiple passes, and simultaneously perform laser scanning under the protection of protective gas until the laser cladding alloy powder layer clad on the mold surface reaches a thickness of 2 to 3 mm.
6. A method for using the laser cladding alloy powder for the surface of mold steel as claimed in claim 5, Features: When the laser scans the same layer, it is in the same direction as the laying of the cladding powder; when laying another layer, the scanning is performed at a rotation angle.
7. A method for using the laser cladding alloy powder for the surface of mold steel as claimed in claim 5, Features: The laser scanner on the selective laser melter can be operated separately from the selective laser melter.
Citation Information
Cited By
Substrate preheating and heat preservation-free superhard corrosion-resistant laser cladding material as well as preparation method, use equipment and use method of substrate preheating and heat preservation-free superhard corrosion-resistant laser cladding material
CN119932439A