Corrosion inhibitor for zinc-aluminum-magnesium coated steel plate, preparation method and composite protective film
The composite corrosion inhibitor of thiazole corrosion inhibitor and polyphosphate and zinc salt is formed to form a composite protective film, which solves the problem of filamentous corrosion on the surface of zinc-aluminum-magnesium-coated steel plate, significantly improves the corrosion inhibition rate and delays the corrosion rate.
Patent Information
- Application Number
- CN202411228349.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The prior art is difficult to effectively suppress the filamentous corrosion of the surface of zinc-aluminum-magnesium-coated steel plates, especially the problem of rapid corrosion expansion in coating defects.
The composite corrosion inhibitor composed of thiazole corrosion inhibitors, polyphosphate and zinc salts, is used to form a composite protective film through the synergistic effect of adsorption and precipitation corrosion inhibitors, and fill it in the molecular voids of the adsorption protective film to enhance the Tightness to inhibit corrosion.
The corrosion inhibition rate of zinc-aluminum-magnesium-coated steel plate surface is significantly improved, the corrosion occurrence time is extended, the corrosion rate is delayed, and the filamentous corrosion is effectively suppressed.
Smart Images

Figure CN119061405A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal surface treatment, and in particular to a corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, a preparation method thereof, and a composite protective film. Background Art
[0002] Zinc-based coating can effectively improve the corrosion resistance of steel surface, especially after adding a small amount of aluminum and magnesium elements to the coating. The addition of aluminum and magnesium elements can effectively refine the grains and form a multiphase structure in the coating, including pure zinc phase, Zn-MgZn2 binary eutectic phase, Zn-MgZn2-Al ternary eutectic phase, etc. Among them, MgZn2 has the lowest corrosion potential and corrodes and dissolves preferentially as an anode. The dissolved MgZn2 phase provides Mg 2+ OH produced by oxygen reduction - The preferential reaction generates Mg(OH)2, which can effectively alleviate the increase in pH and promote the formation of basic zinc salts. The corrosion product is dense and electronically insulating, which can effectively isolate the further invasion of corrosion factors and provide better protection for the steel matrix. Therefore, the zinc-aluminum-magnesium coating has better corrosion resistance.
[0003] However, when steel or aluminum plates are used as coated plates, due to the presence of organic coatings on the surface, when there are defects in the coating, corrosive ions corrode the coating at the damaged position of the paint film, causing local corrosion, and the oxygen concentration difference between the film and the outside environment causes the corrosion to expand rapidly. At present, filamentous corrosion has been found on the surfaces of various materials such as carbon steel, aluminum alloy, and zinc-based coated steel plates. Corrosion inhibitors are one of the most efficient and convenient anti-corrosion methods in the current industrial field. They are chemicals that exist in low concentrations in corrosive media and can effectively slow down or prevent material corrosion. They have the advantages of simple operation, low cost, and significant effects. Corrosion inhibitors are mainly divided into organic corrosion inhibitors and inorganic corrosion inhibitors. Organic corrosion inhibitors mainly contain organic compounds of heteroatoms such as N, P, and S. The lone pair electrons in them are easy to interact with the empty orbits on the metal surface to form an adsorption film and thus play a role in corrosion inhibition. Inorganic corrosion inhibitors mainly include chromates, nitrites, molybdates, borates, phosphates, etc., and their mechanism of action is mainly to react on the metal surface to form a dense oxide film or precipitation film. At present, the research on the inhibitor system for inhibiting filiform corrosion is mainly focused on materials such as carbon steel and aluminum alloy, and there are few reports on the inhibitors for zinc-aluminum-magnesium coating materials. Therefore, it is of great significance to develop an inhibitor system for inhibiting filiform corrosion of zinc-aluminum-magnesium coatings. Summary of the invention
[0004] The present application provides a corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, a preparation method, and a composite protective film to solve the following technical problem: how to inhibit surface filamentous corrosion of zinc-aluminum-magnesium coated steel plates.
[0005] In the first aspect, the present application provides a corrosion inhibitor for zinc-aluminum-magnesium coated steel plates. The components of the corrosion inhibitor include, by mass fraction: solute: 0.1% to 10%, solvent 90% to 99.9%; wherein, by mass fraction, the chemical composition of the solute includes: 30 to 50 parts of thiazole corrosion inhibitor, 30 to 50 parts of polyphosphate, and 5 to 30 parts of zinc salt.
[0006] Optionally, the solvent is a mixed solution of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is (1:5) to (1:20).
[0007] Optionally, the thiazole corrosion inhibitor includes one or more of benzothiazole, mercaptobenzothiazole, benzothiadiazole, sodium mercaptobenzothiazole and sodium thiolbenzothiazole.
[0008] Optionally, the polyphosphate includes one or more of sodium tripolyphosphate and sodium hexametaphosphate.
[0009] Optionally, the zinc salt includes one or more of zinc chloride, zinc nitrate and zinc sulfate.
[0010] Optionally, the components of the corrosion inhibitor include, by mass fraction: solute: 1% to 5%, solvent 95% to 99%; wherein, by mass fraction, the chemical composition of the solute includes: 40 to 50 parts of thiazole corrosion inhibitor, 40 to 50 parts of polyphosphate, and 5 to 15 parts of zinc salt; the solvent is a mixed solution of ethanol and deionized water, and the volume ratio of ethanol to deionized water is 1:5.
[0011] In a second aspect, the present application provides a method for preparing the corrosion inhibitor according to any one embodiment of the first aspect, the method comprising:
[0012] Dissolving a thiazole corrosion inhibitor in ethanol and performing a first stirring to obtain a first solution;
[0013] Dissolving polyphosphate in deionized water and performing a second stirring to obtain a second solution;
[0014] The second solution is added to the first solution, and then the zinc salt is added, and a third stirring is performed to obtain a corrosion inhibitor.
[0015] Optionally, the temperatures of the first stirring, the second stirring and the third stirring are all 20° C. to 50° C., and the times of the first stirring, the second stirring and the third stirring are all 30 min to 60 min.
[0016] In the third aspect, the present application provides a composite protective film, which is formed by the corrosion inhibitor described in any one of the embodiments in the first aspect through adsorption and precipitation reaction, and the composite protective film formed by the corrosion inhibitor has a corrosion inhibition rate of ≥70% for filamentous corrosion of zinc-aluminum-magnesium steel plates.
[0017] Optionally, the composite protective film includes an adsorption-type protective film and a precipitation-type protective film, and the precipitation-type protective film partially fills the molecular gaps of the adsorption-type protective film.
[0018] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0019] The present application discloses a corrosion inhibitor for zinc-aluminum-magnesium coated steel sheet. The components of the corrosion inhibitor include, by mass fraction, solute: 0.1% to 10%, solvent 90% to 99.9%; wherein, by mass fraction, the chemical composition of the solute includes: 30 to 50 parts of thiazole corrosion inhibitor, 30 to 50 parts of polyphosphate, and 5 to 30 parts of zinc salt. The present application rationally designs the components of the corrosion inhibitor, uses thiazole corrosion inhibitor as an adsorption-type corrosion inhibitor, and uses polyphosphate and zinc salt to form a precipitation-type corrosion inhibitor. The adsorption-type corrosion inhibitor and the precipitation-type corrosion inhibitor are compounded. Through the synergistic effect of the adsorption-type corrosion inhibitor and the precipitation-type corrosion inhibitor, an adsorption-type protective film and a precipitation-type protective film are formed. The precipitation-type protective film is partially filled in the molecular voids of the adsorption-type protective film. The composite protective film is denser than a single protective film, thereby greatly improving the corrosion inhibition effect, prolonging the corrosion occurrence time, and delaying the corrosion rate. In this way, the surface filamentous corrosion of the zinc-aluminum-magnesium coated steel sheet is inhibited. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0022] Figure 1 A schematic flow chart of a method for preparing a corrosion inhibitor for zinc-aluminum-magnesium coated steel plates provided in an embodiment of the present application. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0024] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0025] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0026] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0027] The present application provides a corrosion inhibitor for zinc-aluminum-magnesium coated steel plates. The components of the corrosion inhibitor include, by mass fraction: solute: 0.1% to 10%, solvent 90% to 99.9%; wherein, by mass fraction, the chemical composition of the solute includes: 30 to 50 parts of thiazole corrosion inhibitor, 30 to 50 parts of polyphosphate, and 5 to 30 parts of zinc salt.
[0028] In some embodiments, the solvent is a mixed solution of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is (1:5) to (1:20).
[0029] In some embodiments, the thiazole corrosion inhibitor includes one or more of benzothiazole, mercaptobenzothiazole, benzothiadiazole, sodium mercaptobenzothiazole and sodium mercaptobenzothiazole.
[0030] In some embodiments, the polyphosphate includes one or more of sodium tripolyphosphate and sodium hexametaphosphate.
[0031] In some embodiments, the zinc salt includes one or more of zinc chloride, zinc nitrate and zinc sulfate.
[0032] In the above embodiment, the mass fraction of the solute is controlled to be 0.1% to 10%, and the mass fraction of the solvent is 90% to 99.9%. This is because if the solute content is too little, a continuous and dense corrosion inhibitor film layer cannot be formed on the surface of the steel plate, and the corrosion inhibition efficiency is low; if the solute is too much, the corrosion inhibition efficiency will not be significantly improved after the corrosion inhibitor reaches the saturated adsorption amount, and the cost will increase. Exemplarily, in the corrosion inhibitor, the mass fraction of the solute can be 0.1%, 1%, 2%, 3%, 5%, 7%, 9%, 10%, etc., and the mass fraction of the solvent solute is 90%, 91%, 93%, 95%, 97%, 99%, 99.9%, etc.
[0033] In the above embodiment, it should be noted that the solute is composed of thiazole corrosion inhibitor, polyphosphate and zinc salt. The thiazole corrosion inhibitor is controlled to be 30 to 50 parts. This is because the thiazole corrosion inhibitor has a benzene ring structure and atoms such as N and S containing lone pairs of electrons. The benzene ring can increase the adsorption area of the corrosion inhibitor on the surface of the steel plate. At the same time, the phenyl group improves its hydrophobicity and adsorbs on the steel surface to form a hydrophobic film with a large coverage area, thereby improving the corrosion inhibition effect. N and S atoms can provide more adsorption sites, in which the lone pairs of electrons are additionally bonded to the surface of the steel plate to produce strong adsorption, thereby blocking the direct contact between the corrosive medium and the surface of the steel plate and delaying corrosion. Control 30 to 50 parts of polyphosphate and 5 to 30 parts of zinc salt. This is because polyphosphate can bind to Mg on the one hand, and Mg on the other hand. 2+ 、Zn 2+ Metal ions such as zinc, aluminum and magnesium have the ability to generate complexes, polyphosphates can react with metal elements in zinc, aluminum and magnesium coatings, and the present embodiment provides a water-soluble zinc salt with good water solubility, which can be used as a metal ion supplement in the solution, and can also form dense zinc phosphate with polyphosphate, so as to form a precipitation type protective film, increase the surface charge transfer resistance of the coating, and improve corrosion resistance. On the other hand, the polyphosphate ion structure is relatively small, and can be filled in the gaps of macromolecular adsorption films such as thiazoles, and the mixed corrosion inhibitor film is denser than the single corrosion inhibitor film. Exemplary, the solute is composed of the following components, each component is measured by weight, thiazole corrosion inhibitor can be 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, etc., polyphosphate can be 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, etc., and zinc salt can be 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, etc.
[0034] In the above embodiment, the volume ratio of ethanol and deionized water in the solvent is controlled to be ethanol: deionized water = (1:5) to (1:20). If the ethanol content is too low, the thiazole corrosion inhibitor cannot be completely dissolved. If the ethanol content is too high, the solvent is easy to evaporate during the preparation and stirring process. Exemplarily, the volume ratio of ethanol and deionized water can be 1:5, 1:8, 1:10, 1:12, 1:15, 1:18, 1:20, etc.
[0035] In some embodiments, the components of the corrosion inhibitor include, by mass fraction: solute: 1% to 5%, solvent 95% to 99%; wherein, by mass fraction, the chemical composition of the solute includes: 40 to 50 parts of thiazole corrosion inhibitor, 40 to 50 parts of polyphosphate, and 5 to 15 parts of zinc salt, and the solvent is a mixed solution of ethanol and deionized water, and the volume ratio of ethanol to deionized water is 1:5.
[0036] Figure 1 A schematic flow chart of a method for preparing a corrosion inhibitor for zinc-aluminum-magnesium coated steel plates provided in an embodiment of the present application.
[0037] See also Figure 1 The present application provides a method for preparing a corrosion inhibitor, the method comprising:
[0038] S1, dissolving the thiazole corrosion inhibitor in ethanol, and performing a first stirring to obtain a first solution;
[0039] S2, dissolving the polyphosphate in deionized water, and performing a second stirring to obtain a second solution;
[0040] S3, adding the second solution to the first solution, then adding zinc salt, and performing a third stirring to obtain a corrosion inhibitor.
[0041] In some embodiments, the temperatures of the first stirring, the second stirring and the third stirring are all 20° C. to 50° C., and the times of the first stirring, the second stirring and the third stirring are all 30 min to 60 min.
[0042] In the above embodiment, the temperature of the first stirring, the second stirring and the third stirring is controlled to be 20℃~50℃. This is because if the stirring temperature is too low, the adsorption and precipitation of the corrosion inhibitor are slow, and a dense corrosion inhibitor film layer cannot be quickly formed on the surface of the steel plate; if the stirring temperature is too high, the organic molecules will be inactivated and the corrosion inhibition efficiency will be reduced. The time of the first stirring, the second stirring and the third stirring is controlled to be 30min~60min. This is because if the stirring time is too short, the corrosion inhibitor will be unevenly mixed, resulting in uneven local adsorption / precipitation reaction; if the stirring time is too long, there is a possibility of complexation reaction between polyphosphate and zinc salt in the corrosion inhibitor solution. Exemplarily, the temperatures of the first stirring, the second stirring and the third stirring can all be 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, etc., and the time of the first stirring, the second stirring and the third stirring can all be 30min, 35min, 40min, 45min, 50min, 55min, 60min, etc.
[0043] The product prepared by the method for preparing the corrosion inhibitor is the above-mentioned corrosion inhibitor. The chemical composition and microstructure of the corrosion inhibitor prepared by the method for preparing the corrosion inhibitor can refer to the above-mentioned embodiment. Since the method for preparing the corrosion inhibitor adopts part or all of the technical solutions of the corrosion inhibitor embodiment, it has at least all the beneficial effects brought by the technical solutions of the corrosion inhibitor embodiment, which will not be repeated here one by one.
[0044] Based on a general inventive concept, the present application provides a composite protective film, which is formed by adsorption and precipitation reaction of a corrosion inhibitor, and the composite protective film formed by the corrosion inhibitor has a corrosion inhibition rate of ≥70% for filamentous corrosion of zinc-aluminum-magnesium steel plates.
[0045] In some embodiments, the composite protective film includes an adsorption-type protective film and a precipitation-type protective film, and the precipitation-type protective film partially fills the molecular gaps of the adsorption-type protective film.
[0046] The present application compounds an adsorption type corrosion inhibitor with a precipitation type corrosion inhibitor, and through the synergistic effect of the adsorption type corrosion inhibitor and the precipitation type corrosion inhibitor, an adsorption type protective film and a precipitation type protective film are formed, and the precipitation type protective film is filled in the molecular gaps of the adsorption type protective film, thereby greatly improving the corrosion inhibition effect, prolonging the corrosion occurrence time, and slowing down the corrosion rate.
[0047] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0048] Example 1
[0049] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 0.2wt% of the corrosion inhibitor, and the solvent accounts for 99.8wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 50 parts of benzothiazole, 40 parts of sodium tripolyphosphate, and 10 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0050] The preparation method comprises the following steps: (1) dissolving benzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 25° C., and the stirring time is 60 minutes.
[0051] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 70%.
[0052] Example 2
[0053] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 5wt% of the corrosion inhibitor and the solvent accounts for 95wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 50 parts of mercaptobenzothiazole, 40 parts of sodium hexametaphosphate, and 10 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0054] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium hexametaphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 25° C., and the stirring time is 30 minutes.
[0055] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 90%.
[0056] Example 3
[0057] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 0.5wt% of the corrosion inhibitor, and the solvent accounts for 99.5wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 45 parts of mercaptobenzothiazole, 40 parts of sodium tripolyphosphate, and 5 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0058] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 25° C., and the stirring time is 30 minutes.
[0059] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 80%.
[0060] Example 4
[0061] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor, and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 40 parts of benzothiadiazole, 50 parts of sodium tripolyphosphate, and 10 parts of zinc nitrate; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0062] The preparation method comprises the following steps: (1) dissolving benzothiadiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc nitrate, and stirring until the solution is fully mixed. The stirring temperature is 25° C., and the stirring time is 30 minutes.
[0063] The corrosion inhibitor was dripped onto the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 88%.
[0064] Example 5
[0065] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 1wt% of the corrosion inhibitor and the solvent accounts for 99wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 40 parts of sodium mercaptobenzothiazole, 50 parts of sodium hexametaphosphate, and 10 parts of zinc nitrate; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:10.
[0066] The preparation method comprises the following steps: (1) dissolving sodium mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 11 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 10 / 11 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc nitrate, and stirring until the solution is fully mixed. The stirring temperature is 25° C., and the stirring time is 30 minutes.
[0067] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 84%.
[0068] Example 6
[0069] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor, and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 40 parts of sodium thiol benzothiazole, 50 parts of sodium tripolyphosphate, and 10 parts of zinc sulfate; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:10.
[0070] The preparation method comprises the following steps: (1) dissolving sodium thiol benzothiazole in ethanol with a solvent ratio of 1 / 11 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 10 / 11 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc sulfate, and stirring until the solution is fully mixed. The stirring temperature is 25° C., and the stirring time is 30 minutes.
[0071] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 86%.
[0072] Example 7
[0073] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor, and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 45 parts of mercaptobenzothiazole, 45 parts of sodium tripolyphosphate, and 10 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0074] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 25° C., and the stirring time is 30 minutes.
[0075] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 89%.
[0076] Example 8
[0077] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor, and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 45 parts of mercaptobenzothiazole, 45 parts of sodium tripolyphosphate, and 10 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0078] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 40° C., and the stirring time is 30 minutes.
[0079] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 93%.
[0080] Comparative Example 1
[0081] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is mercaptobenzothiazole and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0082] The preparation method comprises the following steps: dissolving mercaptobenzothiazole in a solvent and stirring until the mercaptobenzothiazole is completely dissolved at a stirring temperature of 40° C. and a stirring time of 30 minutes.
[0083] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 44%.
[0084] Comparative Example 2
[0085] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components: sodium tripolyphosphate and zinc chloride, the mass ratio of sodium tripolyphosphate to zinc chloride is 9:2; the solvent is a mixed solution of ethanol and deionized water, the volume ratio is 1:5.
[0086] The preparation method comprises the following steps: dissolving sodium tripolyphosphate and zinc chloride in a solvent, stirring until completely dissolved, stirring at a temperature of 40° C., and stirring for 30 minutes.
[0087] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 35%.
[0088] Comparative Example 3
[0089] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 89 parts of mercaptobenzothiazole, 9 parts of sodium tripolyphosphate, and 2 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0090] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 40° C., and the stirring time is 30 minutes.
[0091] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 58%.
[0092] Comparative Example 4
[0093] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 78 parts of mercaptobenzothiazole, 18 parts of sodium tripolyphosphate, and 4 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0094] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 40° C., and the stirring time is 30 minutes.
[0095] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 54%.
[0096] Comparative Example 5
[0097] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 56 parts of mercaptobenzothiazole, 36 parts of sodium tripolyphosphate, and 8 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0098] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 40° C., and the stirring time is 30 minutes.
[0099] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 48%.
[0100] Comparative Example 6
[0101] A corrosion inhibitor for zinc-aluminum-magnesium coated steel plates, the corrosion inhibitor comprising a solute and a solvent, wherein the solute accounts for 2wt% of the corrosion inhibitor and the solvent accounts for 98wt% of the corrosion inhibitor; wherein the solute is composed of the following components, each component is measured in parts by weight: 34 parts of mercaptobenzothiazole, 54 parts of sodium tripolyphosphate, and 12 parts of zinc chloride; and the solvent is a mixed solution of ethanol and deionized water, with a volume ratio of 1:5.
[0102] The preparation method comprises the following steps: (1) dissolving mercaptobenzothiazole in ethanol with a solvent ratio of 1 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (2) dissolving sodium tripolyphosphate in deionized water with a solvent ratio of 5 / 6 to prepare a solution of a certain concentration, and stirring until the solution is completely dissolved; (3) slowly adding the solution obtained in (2) to the mixed solution obtained in (1), adding zinc chloride, and stirring until the solution is fully mixed. The stirring temperature is 40° C., and the stirring time is 30 minutes.
[0103] The corrosion inhibitor was added dropwise to the defective position of the coating. Through experimental tests, the corrosion inhibition rate of the corrosion inhibitor on the filamentary corrosion of the zinc-aluminum-magnesium plate was 56%.
[0104] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0105] In the embodiments of the present invention, the corrosion inhibition efficiency is high, and the adsorption type corrosion inhibitor and the precipitation type corrosion inhibitor are compounded to greatly improve the corrosion inhibition effect, prolong the corrosion occurrence time, and slow down the corrosion rate.
[0106] In the embodiments of the present invention, the preparation method of the corrosion inhibitor is simple, the cost is low, the dosage is small, the toxicity is low, and there is no secondary pollution to the environment.
[0107] In the embodiment of the present invention, the corrosion inhibitor system has no effect on the surface morphology and appearance of the steel plate, and does not affect other subsequent properties. Therefore, the present invention has a good application prospect in inhibiting the filiform corrosion of zinc, aluminum and magnesium materials.
[0108] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A corrosion inhibitor for zinc-aluminum-magnesium coated steel sheet, characterized in that: Calculated by mass fraction, the components of the corrosion inhibitor include: solute: 0.1% to 10%, solvent 90% to 99.9%; wherein, calculated by mass, the chemical composition of the solute includes: 30 to 50 parts of thiazole corrosion inhibitor, 30 to 50 parts of polyphosphate, and 5 to 30 parts of zinc salt.
2. The corrosion inhibitor according to claim 1, characterized in that The solvent is a mixed solution of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is (1:5) to (1:20).
3. The corrosion inhibitor according to claim 1, characterized in that The thiazole corrosion inhibitor includes one or more of benzothiazole, mercaptobenzothiazole, benzothiadiazole, sodium mercaptobenzothiazole and sodium thiolbenzothiazole.
4. The corrosion inhibitor according to claim 1, characterized in that The polyphosphate includes one or more of sodium tripolyphosphate and sodium hexametaphosphate.
5. The corrosion inhibitor according to claim 1, characterized in that The zinc salt includes one or more of zinc chloride, zinc nitrate and zinc sulfate.
6. The corrosion inhibitor according to claim 1, characterized in that Calculated by mass fraction, the components of the corrosion inhibitor include: solute: 1% to 5%, solvent 95% to 99%; wherein, calculated by mass, the chemical composition of the solute includes: 40 to 50 parts of thiazole corrosion inhibitor, 40 to 50 parts of polyphosphate, and 5 to 15 parts of zinc salt; the solvent is a mixed solution of ethanol and deionized water, and the volume ratio of ethanol to deionized water is 1:
5.
7. A method for preparing the corrosion inhibitor according to any one of claims 1 to 6, characterized in that: The method comprises: Dissolving a thiazole corrosion inhibitor in ethanol and performing a first stirring to obtain a first solution; Dissolving polyphosphate in deionized water and performing a second stirring to obtain a second solution; The second solution is added to the first solution, and then the zinc salt is added, and a third stirring is performed to obtain a corrosion inhibitor.
8. The method according to claim 7, characterized in that The temperatures of the first stirring, the second stirring and the third stirring are all 20° C. to 50° C., and the times of the first stirring, the second stirring and the third stirring are all 30 min to 60 min.
9. A composite protective film, characterized in that: The composite protective film is formed by the corrosion inhibitor described in any one of claims 1 to 6 through adsorption and precipitation reaction, and the composite protective film formed by the corrosion inhibitor has a corrosion inhibition rate of ≥70% for filamentous corrosion of zinc-aluminum-magnesium steel plates.
10. The composite protective film according to claim 9, characterized in that: The composite protective film comprises an adsorption type protective film and a precipitation type protective film, and the precipitation type protective film is partially filled in the molecular gaps of the adsorption type protective film.
Citation Information
Patent Citations
Multi-component corrosion and scale inhibitor
CN104609579A
Composite corrosion and scale inhibitor and its preparation method and use
CN105565513A
Special passivator for environment-friendly chromium-free galvanized aluminum-magnesium steel plate and passivation process
CN114774905A
Corrosion inhibitor for inhibiting electrochemical corrosion and preparation method thereof
CN116623186A
Device und method for controlling corrosion of cooling water system for terracedie
CN1814558A
Cited By
Special low-film-thickness chromium-free fingerprint-resistant coating for hot-dip galvanizing, aluminum and magnesium
CN121045937A