Preparation method and application of Mo-doped Ni5Se5 electro-catalysis nano material
The preparation of Mo-Ni5Se5 electrocatalytic nanomaterials by sonication and tube furnace calcination combined with ion exchange method has solved the problems of long production time and high energy consumption in the prior art, significantly improved the electrocatalytic performance, and was suitable for industrial applications.
Patent Information
- Application Number
- CN202411349463.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing preparation method of Mo-doped Ni0.85Se electrocatalyst is time-consuming and energy-consuming, and is difficult to control during large-scale production, which limits the yield of Ni0.85Se.
Ultrasonic treatment is used to remove the oxide layer on the surface of the foam nickel, and the Mo-Ni5Se5 electrocatalytic nanomaterial is prepared by tube furnace calcination and ion exchange method to form a three-dimensional pore structure, avoiding the use of reducing gas to control the reaction process.
The porosity of Mo-Ni5Se5 electrocatalytic material has been improved, and its hydrogen evolution reaction (HER) and oxygen evolution reaction (OER) performance has been significantly improved. The preparation method is simple and environmentally friendly, and it is suitable for industrial production.
Smart Images

Figure CN119061428A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalytic materials and relates to a preparation method and application of a Mo-doped Ni5Se5 electrocatalytic nanomaterial. Background Art
[0002] Due to the increasingly severe energy and environmental problems, the development and utilization of clean and sustainable energy has received widespread attention at home and abroad. Clean energy is greatly affected by the natural environment and often cannot provide stable and reliable power input to the national power grid. Therefore, we need to carry out energy conversion to solve the storage and transportation problems of these clean energies. Using electricity generated by clean energy to electrocatalyze water to decompose water to produce hydrogen is one of the effective means to achieve clean electricity conversion, storage and transportation. In addition, with the rapid development of the hydrogen fuel cell industry, the demand for hydrogen will increase day by day. Compared with traditional chemical hydrogen production solutions such as methane, methanol, and coal, electrocatalytic water decomposition to produce hydrogen can provide cleaner hydrogen fuel and effectively solve the poisoning of residual carbon-containing small molecules to fuel cell catalysts.
[0003] To date, the mainstream catalysts for water electrolysis are still mainly precious metal catalysts such as Pt / C, RuO2, and IrO2, which greatly increases the cost of hydrogen production and severely limits the large-scale use of hydrogen energy. In contrast, molybdenum, as a common and inexpensive transition metal material, is also widely used in the field of electrocatalytic hydrogen production. In recent years, molybdenum-based catalysts have received widespread attention as new electrocatalyst materials. Compared with other common metal catalysts, molybdenum-based compounds have higher chemical stability and greater chemical conductivity. In addition, molybdenum-based compounds have adjustable conductivity, surface area, and surface chemical activity, which enable them to exhibit excellent electrocatalytic performance in water electrolysis reactions.
[0004] Nickel selenide exhibits good electrocatalytic activity at low overpotentials and has a high cathode current density. Therefore, the construction of molybdenum-doped nickel selenide nanomaterials and the study of their water electrolysis performance are of great significance and value in the fields of materials science and energy research.
[0005] Although there is a kind of Mo doped Ni in the prior art, CN116876025A discloses 0 .85 Se electrocatalyst and its preparation method and application. However, it is necessary to firstly perform a hydrothermal reaction in nickel foam and grow Mo-MOF material on the surface of nickel foam, which not only takes a long time, but also consumes a lot of energy when produced in large quantities. More importantly, in the subsequent steps, inert gas and reducing protective gas need to be added, and the progress of the reaction is difficult to control, which ultimately limits the yield of Ni0.85Se. Summary of the invention
[0006] The technical problem to be solved by the present invention is to address the deficiencies in the prior art. The present invention provides a method for preparing a Mo-Ni5Se5 electrocatalytic nanomaterial and an application thereof, wherein the Mo-Ni5Se5 electrocatalytic nanomaterial prepared by the method for preparing the Mo-Ni5Se5 electrocatalytic nanomaterial has a higher porosity and therefore has better HER (hydrogen evolution reaction) and OER (oxygen evolution reaction) performance.
[0007] In order to achieve the above advantages, the present invention provides a method for preparing a Mo-Ni5Se5 electrocatalytic nanomaterial, the method comprising the following steps: S1001, subjecting the nickel foam (NF) to ultrasonic treatment in a pretreatment solution to remove a surface oxide layer, and after the surface oxide layer is removed by ultrasonic treatment, washing with a cleaning solution, and placing the cleaned (NF) in a vacuum oven to dry, thereby obtaining a cleaned nickel foam; S1002, placing selenium powder upstream of the porcelain boat and pretreated nickel foam downstream, then placing the powder in a tube furnace, calcining the tube furnace under the protection of continuous inert gas flow, washing with ethanol and ultrapure water respectively, and drying in a vacuum oven to obtain Ni5Se5 / NF; S1003, soaking Ni5Se5 / NF in an ethanol solution of MoCl5, and then washing with detergents, and drying in a vacuum oven to obtain a Mo-Ni5Se5 / NF nano-electrocatalytic material with a three-dimensional pore structure.
[0008] According to one embodiment of the present invention, the cleaning solution is ethanol and / or pure water, wherein the washing solution is ethanol and / or pure water. According to one embodiment of the present invention, the pretreatment solution is HCl solution, the concentration of the hydrochloric acid solution is 1-3 mol / L, and the ultrasonic treatment time is 10-30 minutes.
[0009] According to an embodiment of the present invention, during the pretreatment, washing is performed by sequentially using ethanol and ultrapure water, and the washing time is 5 to 20 minutes.
[0010] According to an embodiment of the present invention, during the pretreatment, the drying is vacuum drying, the drying temperature is 50-80° C., and the drying time is 8-12 h.
[0011] According to an embodiment of the present invention, in step S1002, the selenization method is high-temperature calcination in a nitrogen atmosphere in a tubular furnace, the calcination temperature is 200-350°C, and the heating rate is 1-3°C min -1 , keep warm for 3-5 hours.
[0012] According to an embodiment of the present invention, the concentration of the MoCl5 ethanol solution is 0.1-1 mol / L. The ion exchange method is soaking in the MoCl5 ethanol solution for 10-30 h.
[0013] In order to achieve at least one of the above advantages, the present invention provides the use of the Mo-Ni5Se5 electrocatalytic nanomaterial, which is used for hydrogen evolution reaction and oxygen evolution reaction.
[0014] Compared with the prior art, the present invention has the following advantages: (1) The Mo-Ni5Se5 prepared by the present invention using the ion exchange method has a three-dimensional porous nanostructure and has a higher electrochemical active area. The prepared Mo-Ni5Se5 has excellent HER and OER performance.
[0015] (2) The Mo-Ni5Se5 electrocatalytic material prepared by the present invention has good cycle performance and will not cause secondary pollution to the environment during application.
[0016] (3) The preparation method of the present invention is easy to operate, has low raw material cost, is environmentally friendly and has the potential for large-scale production, which is conducive to industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is the XRD spectrum of the Mo-Ni5Se5 electrocatalyst prepared in Example 1 of the present invention;
[0018] Figure 2 The SEM photos of the Ni5Se5 and Mo-Ni5Se5 electrocatalyst materials prepared in Example 1 of the present invention are shown;
[0019] Figure 3 Elemental energy spectrum of Mo, Ni and Se of the Mo-Ni5Se5 electrocatalyst prepared in Example 1 of the present invention;
[0020] Figure 4 LSV curves of HER performance of NF, Ni5Se5 and Mo-Ni5Se5 electrocatalysts prepared in Example 1 of the present invention in a 1 M KOH environment;
[0021] Figure 5 The Nyquist plots and C of the catalysts during the HER process of the NF, Ni5Se5 and Mo-Ni5Se5 electrocatalysts prepared in Example 1 of the present invention are shown in FIG. dl ;
[0022] Figure 6 LSV curves of the OER performance of NF, Ni5Se5 and Mo-Ni5Se5 electrocatalysts prepared in Example 1 of the present invention in a 1 M KOH environment;
[0023] Figure 7 The Nyquist plots and C of the catalysts during the OER process of the NF, Ni5Se5 and Mo-Ni5Se5 electrocatalysts prepared in Example 1 of the present invention are shown in FIG. dl ; DETAILED DESCRIPTION
[0024] The preferred embodiments described below are for example only, and those skilled in the art may think of other obvious variations. The basic principles of the present invention defined in the following description may be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.
[0025] In order to achieve at least one of the above advantages, the present invention provides a technical problem to be solved by the present invention. The present invention is aimed at the deficiencies of the prior art. The present invention provides a method for preparing Mo-Ni5Se5 electrocatalytic nanomaterial, and the method comprises the following steps: S1001, subjecting the nickel foam (NF) to ultrasonic treatment in a pretreatment solution to remove a surface oxide layer, and after the surface oxide layer is removed by ultrasonic treatment, washing with a cleaning solution, and placing the cleaned (NF) in a vacuum oven to dry, thereby obtaining a cleaned nickel foam; S1002, placing selenium powder upstream of the porcelain boat and pretreated nickel foam downstream, then placing the powder in a tube furnace, calcining the tube furnace under the protection of continuous inert gas flow, washing with ethanol and ultrapure water respectively, and drying in a vacuum oven to obtain Ni5Se5 / NF; S1003, soaking Ni5Se5 / NF in an ethanol solution of MoCl5, and then washing with detergents, and drying in a vacuum oven to obtain a Mo-Ni5Se5 / NF nano-electrocatalytic material with a three-dimensional pore structure.
[0026] In this way, not only can Mo-doped Ni5Se5 electrocatalytic nanomaterials with higher porosity be obtained, but also the addition of reducing gas can be avoided, thereby controlling the progress of the reaction. In particular, in step S1003, if reducing gas is added, it will react with Ni in the Ni5Se5 / NF material, thereby failing to generate Mo-Ni5Se5 / NF nano electrocatalytic material.
[0027] Preferably, in step S1001, the cleaning liquid is ethanol and / or pure water.
[0028] Also preferably, in step S1001, the washing liquid is ethanol and / or pure water.
[0029] Preferably, the substrate material is nickel foam with a size of 1-2 cm x 2-3 cm.
[0030] Preferably, in step S1001, the pretreatment solution is an HCl solution, the concentration of the hydrochloric acid solution is 1-3 mol / L, and the ultrasonic treatment time is 10-30 minutes.
[0031] Preferably, during the pretreatment, washing is performed by sequentially using ethanol and ultrapure water, and the washing time is 5 to 20 minutes.
[0032] Preferably, during the pretreatment, the drying is vacuum drying, the drying temperature is 50-80° C., and the drying time is 8-12 h.
[0033] In step S1002, the selenization method is high-temperature calcination in a tubular furnace under a nitrogen atmosphere, the calcination temperature is 200-350°C, and the heating rate is 1-3°C min -1 , and keep warm for 3-5 h. Compared with the 55 degrees Celsius per minute in the method disclosed in CN116876025A, the reaction conditions are milder, which is conducive to improving the porosity of the Mo-doped Ni5Se5 finally formed, thereby effectively improving its electrochemical performance.
[0034] The concentration of the MoCl5 ethanol solution is 0.1-1 mol / L. The ion exchange method is soaking in the MoCl5 ethanol solution for 10-30 hours.
[0035] It is worth mentioning that the conventional three-electrode system was used at room temperature with 1.0 M KOH solution as the electrolyte for electrocatalysis and a scan rate of 5 mV s -1 Ag / AgCl (saturated KCl) was used as the reference electrode and the carbon rod was used as the counter electrode. 2 Mo-Ni5Se5 material is the working electrode, and HER and OER reactions occur in the electrolyte.
[0036] Example 1
[0037] 1x3 cm 2 Nickel foam (NF) was ultrasonically treated in 3 mol / L HCl solution for 10 minutes to remove the surface oxide layer. After being taken out, it was washed with ethanol and ultrapure water for 20 minutes respectively. The treated NF was placed in a 60℃ vacuum oven and dried for 8 hours to obtain pretreated NF. 1 g of selenium powder was placed upstream of the porcelain boat, and the treated nickel foam was placed downstream. The ceramic boat was placed in a tube furnace and heated to 300℃ in a tube furnace under continuous N2 flow conditions at a heating rate of 3℃min -1,Keep warm for 3 h, cool to room temperature, wash with ethanol and ultrapure water for 20 minutes respectively, put in a 60 ℃ vacuum oven and dry for 12 hours to obtain Ni5Se5 / NF. Put the Ni5Se5 / NF obtained above into 0.5 mol / L MoCl5 ethanol solution, soak for 24 h, wash with ethanol and ultrapure water for 20 minutes respectively, and dry in a 60 ℃ vacuum oven for 12 hours to obtain Mo-Ni5Se5 electrocatalytic nanomaterials.
[0038] The Mo-Ni5Se5 material obtained in Example 1 was used as the working electrode, graphite as the counter electrode, and Ag / AgCl (saturated KCl) electrode as the reference electrode, connected to Shanghai Chenhua CHI 660E electrochemical workstation, and electrocatalyzed in 1 M KOH electrolyte. -2 The HER and OER overpotentials are 185 mV and 143 mV.
[0039] The X-ray diffraction spectrum (XRD) of the Mo-Ni5Se5 electrocatalyst material prepared in Example 1 is as follows: Figure 1 As shown. Figure 1 It can be seen that only the diffraction peaks of active species Ni (PDF#04-0850) and Ni5Se5 (PDF#71-2279) appear, proving the successful preparation of Ni5Se5. There is no diffraction peak of Mo-related crystal phase, which may be caused by simple Mo doping.
[0040] The SEM image of the Mo-Ni5Se5 electrocatalytic material prepared in Example 1 is as follows: Figure 2 As shown in the figure. The prepared Mo-Ni5Se5 / NF and the precursor Ni5Se5 / NF are both three-dimensional porous nanostructures. This morphology not only increases the specific surface area of the catalyst, but also further improves the hydrophilicity of NF, which is more conducive to the doping of Mo in the subsequent impregnation. The material after ion exchange still maintains this morphology with high specific surface area, which is the key factor to achieve excellent performance.
[0041] The elemental energy spectra of Mo, Ni and Se of the Mo-Ni5Se5 electrocatalyst prepared in Example 1 are as follows: Figure 3 As shown, in order to determine the distribution of Mo, Ni and Se elements in the prepared samples, elemental analysis of the materials was carried out to confirm the uniform distribution of Mo, Ni and Se elements in Mo-Ni5Se5.
[0042] The LSV curve of the HER performance of the Mo-Ni5Se5 electrocatalyst material prepared in Example 1 in a 1 M KOH environment is as follows: Figure 4 The Mo-Ni5Se5 electrode exhibits an overpotential of 185 mV (10 mA cm-2 ), which is 211 mV lower than the transition point of the precursor Ni5Se5. In order to clarify the source of this high catalytic activity, electrochemical impedance spectroscopy (EIS) and electrochemical active area studies were performed on the Mo-Ni5Se5 electrode, such as Figure 5 The double layer capacitance (C dl Compared with NF and Ni5Se5, Mo-Ni5Se5 exhibits the largest double-layer capacitance (150 mF cm -2 ), which indicates that it has a relatively large electrochemical surface area. To further probe the intrinsic activity of the electrocatalyst, electrochemical impedance spectroscopy (EIS) measurements were performed at an overpotential of 10 mV. The charge transfer resistance (Rct) is related to the electrocatalytic kinetics at the interface between the electrolyte and the electrocatalyst. Generally speaking, the smaller the Rct value, the faster the electron transfer. The Nyquist plot shows that the charge transfer resistance (Rct) of Mo-Ni5Se5 (1 Ω) is much smaller than that of NF and Ni5Se5, indicating that the composite material has a higher conductivity.
[0043] The electrocatalytic material of Mo-Ni5Se5 prepared in Example 1 was tested for its OER catalytic activity in a 1.0 M KOH electrolyte using a typical three-electrode system. In order to eliminate the influence of the capacitive current generated by the oxidation of nickel ions on the catalytic performance, Figure 6 The Mo-Ni5Se5 electrode exhibits an overpotential of 143 mV (10 mA cm -2 ), which is 172 mV lower than the transition point of the precursor Ni5Se5. In order to clarify the source of this high catalytic activity, electrochemical impedance spectroscopy (EIS) and electrochemical active area studies were carried out on the Mo, Mn-NiFe2O4 electrode, such as Figure 7 The double layer capacitance (C dl Compared with NF and Ni5Se5, Mo-Ni5Se5 exhibits the largest double-layer capacitance (222.71 mF cm -2 ), which indicates that it has a relatively large electrochemical surface area. To further probe the intrinsic activity of the electrocatalyst, electrochemical impedance spectroscopy (EIS) measurements were performed at an overpotential of 10 mV. The charge transfer resistance (Rct) is related to the electrocatalytic kinetics at the interface between the electrolyte and the electrocatalyst. Generally speaking, the smaller the Rct value, the faster the electron transfer. The Nyquist plot shows that the charge transfer resistance (Rct) of Mo-Ni5Se5 (0.45 Ω) is much smaller than that of NF and Ni5Se5, indicating that the composite material has a higher conductivity.
[0044] Example 2
[0045] 2x2 cm2 Nickel foam (NF) was ultrasonically treated in 1 mol / L HCl solution for 30 minutes to remove the surface oxide layer. After being taken out, it was washed with ethanol and ultrapure water for 10 minutes respectively. The treated NF was placed in a vacuum oven at 80℃ and dried for 10 hours to obtain pretreated NF. 1 g of selenium powder was placed upstream of the porcelain boat, and the treated nickel foam was placed downstream. The boat was placed in a tube furnace and heated to 200℃ in a tube furnace under continuous N2 flow conditions at a heating rate of 2℃ min -1, Keep warm for 5 h, cool to room temperature, wash with ethanol and ultrapure water for 10 minutes respectively, put in a vacuum oven at 80 °C and dry for 10 hours to obtain Ni5Se5 / NF. Put the Ni5Se5 / NF obtained above into 1 mol / L MoCl5 ethanol solution, soak for 12 h, wash with ethanol and ultrapure water for 10 minutes respectively, and dry in a vacuum oven at 80 °C for 8 hours to obtain porous Mo-Ni5Se5 electrocatalytic nanomaterials.
[0046] The Mo-Ni5Se5 material obtained in Example 2 was used as the working electrode, graphite as the counter electrode, and Ag / AgCl (saturated KCl) electrode as the reference electrode, connected to Shanghai Chenhua CHI 660E electrochemical workstation, and electrocatalyzed in 1 M KOH electrolyte. -2 The HER and OER overpotentials are 193 mV and 155 mV.
[0047] Comparative Example 1 2x2 cm 2 Nickel foam (NF) was ultrasonically treated in 3 mol / L HCl solution for 10 minutes to remove the surface oxide layer. After being taken out, it was washed with ethanol and ultrapure water for 20 minutes respectively. The treated NF was placed in a 60°C vacuum oven and dried for 8 hours to obtain pretreated NF. 1 g of selenium powder was placed upstream of the porcelain boat, and the nickel foam treated in step (1) was placed downstream. They were placed in a tube furnace and heated to 300°C in the tube furnace under continuous N2 flow conditions at a heating rate of 3°C min -1, Keep warm for 3 h, cool to room temperature, wash with ethanol and ultrapure water for 20 min respectively, put into a 60 °C vacuum oven and dry for 12 h to obtain Ni5Se5 / NF.
[0048] The Ni5Se5 / NF material obtained in Comparative Example 1 was used as the working electrode, graphite as the counter electrode, and Ag / AgCl (saturated KCl) electrode as the reference electrode. The material was connected to a Shanghai Chenhua CHI 660E electrochemical workstation and electrocatalyzed in 1M KOH electrolyte.-2 The HER and OER overpotentials are 211 mV and 172 mV.
[0049] The present invention provides a method and idea for preparing a Mo-doped Ni5Se5 electrocatalytic material. There are many methods and approaches to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented using existing technologies.
[0050] It should be understood by those skilled in the art that the embodiments of the present invention described above are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.
Claims
1. Mo-Ni 5 Se 5 Method for preparing electrocatalytic nanomaterials, It is characterized in that The method comprises the following steps: S1001, subjecting the nickel foam (NF) to ultrasonic treatment in a pretreatment solution to remove a surface oxide layer, and after the surface oxide layer is removed by ultrasonic treatment, washing with a cleaning solution, and placing the cleaned (NF) in a vacuum oven to dry, thereby obtaining a cleaned nickel foam; S1002, placing selenium powder upstream of the porcelain boat and pretreated nickel foam downstream, then placing them in a tube furnace, calcining them in the tube furnace under the protection of continuous inert gas flow, washing them with ethanol and ultrapure water respectively, and drying them in a vacuum oven to obtain Ni 5 Se 5 / NF; S1003, Ni 5 Se 5 / NF put into MoCl 5 The Mo-Ni with three-dimensional pore structure can be obtained by immersing the mixture in an ethanol solution and then washing with a washing liquid and drying in a vacuum oven. 5 Se 5 / NF nano-electrocatalytic materials.
2. Mo-Ni according to claim 1 5 Se 5 Method for preparing electrocatalytic nanomaterials, It is characterized in that The cleaning liquid is ethanol and / or pure water, wherein the washing liquid is ethanol and / or pure water.
3. Mo-Ni according to claim 1 5 Se 5 Method for preparing electrocatalytic nanomaterials, It is characterized in that The pretreatment solution is HCl solution, the concentration of the hydrochloric acid solution is 1-3 mol / L, and the ultrasonic treatment time is 10-30 minutes.
4. Mo-Ni according to claim 1 5 Se 5 Method for preparing electrocatalytic nanomaterials, It is characterized in that During pretreatment, washing is performed using ethanol and ultrapure water in sequence, and the washing time is 5 to 20 minutes.
5. Mo-Ni according to claim 1 5 Se 5 Method for preparing electrocatalytic nanomaterials, It is characterized in that During pretreatment, the drying is performed under vacuum, the drying temperature is 50-80°C, and the drying time is 8-12 h.
6. Mo-Ni according to claim 1 5 Se 5 Method for preparing electrocatalytic nanomaterials, It is characterized in that In step S1002, the selenization method is high-temperature calcination in a tubular furnace under a nitrogen atmosphere, the calcination temperature is 200-350°C, and the heating rate is 1-3°C min -1 , keep warm for 3-5 hours.
7. Mo-Ni according to claim 1 5 Se 5 Method for preparing electrocatalytic nanomaterials, It is characterized in that MoCl 5 The concentration of the ethanol solution is 0.1~1 mol / L. The ion exchange method is MoCl 5 Soak in ethanol solution for 10 to 30 hours.
8. Mo-Ni according to any one of claims 1 to 7 5 Se 5 Application of electrocatalytic nanomaterials, It is characterized in that It is used for hydrogen evolution reaction and oxygen evolution reaction.
9. Mo-Ni 5 Se 5 Electrocatalytic nanomaterial, characterized in that it is made by any one of the Mo-Ni described in claims 1 to 7 5 Se 5 The invention is made by the method for preparing electrocatalytic nanomaterials.