Preparation method of composite photo-anode for photoelectrocatalytic hydrogen production, composite photo-anode and application of composite photo-anode
By loading FeMOFs and Co4(μ3-O)4X catalyst on the BiVO4 photoanode, the composite photoanode is solved, and the problem of slow carrier recombination and water oxidation kinetics is significantly improved, and the photoelectrocatalytic performance and stability are achieved. Efficient photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202410971237.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-03
AI Technical Summary
BiVO4 photoanode carriers are easy to recombine, the water oxidation kinetics are slow and the stability is poor, resulting in unsatisfactory photocurrent density.
FeMOFs cocatalyst is loaded on the BiVO4 film by hydrothermal method, and Co4(μ3-O)4X molecular catalyst is introduced on its surface to form BiVO4/FeMOFs@Co4(μ3-O)4X composite photoanode, and FeMOFs are used to provide active sites And inhibits the leaching of V5+, Co4(μ3-O)4X provides OER reactive sites, enhancing electrode stability and catalytic performance.
The efficiency and stability of photoelectrocatalytic decomposition of water is significantly improved, and the photocurrent density reaches more than 3.5 times that of pure BiVO4 electrodes, significantly enhancing PEC performance.
Smart Images

Figure CN119061432A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photoelectrocatalytic materials, and in particular relates to a preparation method of a composite photoanode for photoelectrocatalytic hydrogen production, a composite photoanode and applications thereof. Background Art
[0002] As of January 2024, the world population has exceeded 8.1 billion, and by the middle of this century, it will be close to 10 billion. As the population increases, the demand for energy will increase. As the world's second most populous country, my country's dependence on energy is extremely serious. The combustion of traditional energy will produce a large amount of CO2. At present, my country is implementing the "dual carbon policy". In order to ensure and complete the peak of carbon emissions in 2030 and achieve carbon neutrality before 2060, it is urgent to find new clean energy.
[0003] The photoelectrochemical (PEC) reaction of decomposing water to produce hydrogen is considered to be a promising energy conversion pathway. The water oxidation reaction in PEC water splitting is a complex four-proton coupled multi-electron process and is the rate-determining step of water splitting. Therefore, the development of a photoanode with excellent performance has important basic significance and research value.
[0004] BiVO4 is an excellent candidate for photoanode. Its bandgap width (2.4eV-2.5eV) and long carrier lifetime of 40ns make it particularly suitable for water splitting. However, the hole diffusion span of BiVO4 photoanode is short, only about 70nm, carriers are easy to recombine, and water oxidation kinetics are slow. These shortcomings make the photocurrent density of BiVO4 less than ideal. In order to solve the above problems, the method of loading co-catalysts is usually adopted to solve the problem of slow OER kinetics by promoting the transfer of photogenerated holes, reducing the recombination of photogenerated carriers and reducing the overpotential of surface OER.
[0005] Comparative Publication 1: A method for preparing a ZnO / BiVO4 heterojunction photoanode composite material for photoelectrochemical water splitting (Patent Publication No. CN 110373680A). This patent improves the separation of carriers by constructing a ZnO / BiVO4 heterojunction, synthesizes a BiVO4 film on FTO by electrodeposition, and then loads ZnO on the BiVO4 film using a hydrothermal method. The formation of the ZnO / BiVO4 heterojunction solves the problem of easy recombination of BiVO4 bulk charges to a certain extent. However, the formation of the heterojunction will bring more defects at the interface between the photogenerated semiconductor material and the load material, making the interface a new recombination center for carriers, and cannot further improve the PEC performance of the BiVO4 photoelectric level.
[0006] Comparative Publication 2: A MOFs-coated OV-BiVO4 composite photoanode and its preparation method and application (CN110983362A). This patent first synthesizes BiVO4 nanoarrays by electrochemical deposition-heat treatment, then calcines BiVO4 in a hydrogen environment to form oxygen vacancies, and finally uses a solvothermal method to load MOF materials on OV-BiVO4 after surface anionization treatment. The loading of MOFs can quickly export holes from the OV-BiVO4 interface on the one hand, and on the other hand, it can also protect oxygen vacancies from being eroded by external conditions and enhance the stability of the photoelectric level. However, the ability of the co-catalyst to improve the water oxidation kinetics on the surface of the material is insufficient, and the water oxidation kinetics is still relatively slow. The main reason is that the loading of MOF will also introduce additional recombination centers, which leads to poor interaction between the photoanode and MOF interface, hindering the participation of photogenerated holes in the surface catalysis of water oxidation reaction.
[0007] Compare with the third patent disclosure: a preparation method and application of a BiVO4 / Ni MOF / Co-Pi composite photoanode (CN115747829A). This patent uses the impregnation method to load the Ni MOF material onto the surface of the BiVO4 photoanode to synthesize the BiVO4 / Ni MOF composite photoanode, and then uses the electrodeposition method to deposit a layer of Co-Pi co-catalyst on the outer layer of the BiVO4 / Ni MOF composite photoanode to successfully prepare the BiVO4 / Ni MOF / Co-Pi composite photoanode. The loading of the composite co-catalyst improves the separation of carriers and improves the water oxidation capacity. However, the carrier lifetime of the material itself is short, the migration rate is still slow, and the bulk recombination problem is still serious, resulting in the final photocurrent density still not reaching the ideal level, and the stability time of the electrode must be further extended.
[0008] Therefore, it is urgent to develop a new type of photoelectrocatalytic material that can quickly extract photogenerated holes, accelerate the carrier migration rate, and improve the kinetic characteristics and stability of the OER reaction. Summary of the invention
[0009] In order to solve the problems of easy recombination of BiVO4 photoanode carriers, slow water oxidation kinetics and poor stability, the present invention provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production. The composite photoanode prepared by the method achieves relatively excellent photoelectric conversion efficiency in photoelectrocatalytic water decomposition and has efficient and stable PEC water oxidation performance.
[0010] The present invention also provides a composite photoanode for photoelectrocatalytic hydrogen production and application thereof.
[0011] The present invention is achieved through the following technical solutions:
[0012] The present invention provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production, the preparation method comprising:
[0013] Dissolve FeCl3 and H2ATA (2-aminoterephthalic acid) in DMF solution to obtain a mixed solution;
[0014] Placing the BiVO4 photoanode in the mixed solution for hydrothermal reaction to obtain a BiVO4 / FeMOFs photoanode;
[0015] Co(NO3)2 and CH3CO2Na are dissolved in an organic solvent, and when heated to a specified temperature, a pyridine solution is added, followed by a hydrogen peroxide solution, and the mixture is stirred at reflux temperature until the color of the mixture changes from purple to dark green, thereby obtaining Co4(μ3-O)4X;
[0016] The BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X, and then taken out and dried to obtain a composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X.
[0017] Among them, X in Co4(μ3-O)4X represents (μ-O2CMe)4(py)4·0.5NaNO3·8H2O(1a·0.5NaNO3·8H2O).
[0018] Further, the FeCl3 and H2ATA are dissolved in a DMF solution to obtain a mixed solution, specifically comprising:
[0019] Dissolving FeCl3 and H2ATA together in a DMF solution to obtain a mixed solution;
[0020] Wherein, the molar ratio of FeCl3 and H2ATA in the mixed solution is (1-3):4;
[0021] The molar concentration of FeCl3 in the mixed solution is 0.003-0.005 mol / L;
[0022] The DMF solution is prepared by mixing DMF and water in a volume ratio of 1:1.
[0023] Furthermore, placing the BiVO4 photoanode in the mixed solution for hydrothermal reaction to obtain the BiVO4 / FeMOFs photoanode specifically includes:
[0024] The BiVO4 photoanode is placed in the mixed solution, and subjected to a hydrothermal reaction at 90-120° C. for 18-24 hours. After the hydrothermal reaction is completed, the photoanode is washed and dried to obtain a BiVO4 / FeMOFs photoanode.
[0025] Preferably, the hydrothermal reaction temperature is 90° C. and the reaction time is 20 h.
[0026] Furthermore, the method comprises dissolving Co(NO3)2 and CH3CO2Na in an organic solvent, adding a pyridine solution when heated to a specified temperature, and then adding a hydrogen peroxide solution, and stirring the reaction at a reflux temperature until the color of the mixture changes from purple to dark green to obtain Co4(μ3-O)4X, which specifically comprises:
[0027] Dissolve Co(NO3)2 and CH3CO2Na in methanol, add pyridine solution when heated to 90±5℃, then slowly add hydrogen peroxide solution, stir and react at 90±5℃ for 4-5h until the color of the mixture changes from purple to dark green, and obtain a mixture containing Co4(μ3-O)4X;
[0028] The Co4(μ3-O)4X-containing mixture is stored at room temperature for 3 to 5 days to obtain powdered Co4(μ3-O)4X.
[0029] Preferably, the designated temperature and the reflux temperature are both 90° C.; the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30%; and the mass fraction of pyridine in the pyridine solution is 99%.
[0030] Further, the molar ratio of the Co(NO3)2 and the CH3CO2Na is (1-2):(2-4);
[0031] The molar ratio of the Co(NO3)2 to the pyridine in the pyridine solution is (8-12):1;
[0032] The molar ratio of the Co(NO3)2 to the hydrogen peroxide in the hydrogen peroxide solution is 1:(6-10).
[0033] Furthermore, the BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X, and then taken out and dried to obtain a composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X, which specifically includes:
[0034] The BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X for 5 to 60 minutes, and then taken out and dried at room temperature to obtain a composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X;
[0035] Wherein, in the aqueous solution of Co4(μ3-O)4X, the concentration of Co4(μ3-O)4X is 0.5-5 mg / mL.
[0036] Preferably, the BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X for 20 min; in the aqueous solution of Co4(μ3-O)4X, the concentration of Co4(μ3-O)4X is 1 mg / mL.
[0037] Optionally, the preparation method of the BiVO4 photoanode is as follows:
[0038] Dissolve Bi(NO3)2 and KI in water, then add concentrated nitric acid to adjust the pH to 1.7 to obtain solution A;
[0039] Dissolve p-benzoquinone in anhydrous ethanol to obtain solution B;
[0040] Mixing the A solution and the B solution to obtain a precursor electrolyte;
[0041] Using the precursor electrolyte as a raw material, electrodepositing a BiOI film on the surface of FTO glass;
[0042] A vanadium precursor solution is dropped onto the surface of the BiOI film, and then calcined at 450° C. to obtain a BiVO4 film;
[0043] The BiVO4 film is immersed in a sodium hydroxide solution to obtain a BiVO4 photoanode.
[0044] Furthermore, the process of using the precursor electrolyte as a raw material to electrodeposit a BiOI film on the surface of the FTO glass specifically includes:
[0045] The precursor electrolyte was used as a raw material, FTO glass was used as a working electrode, Ag / AgCl electrode and Pt electrode were used as a reference electrode and a counter electrode, respectively, to electro-deposit a BiOI film, the applied voltage was -0.1 V, and the deposition time was 180 s;
[0046] The step of dripping a vanadium precursor solution on the surface of the BiOI film and then calcining at 450° C. to obtain a BiVO4 film specifically includes:
[0047] A vanadium precursor solution is dripped onto the surface of the BiOI film, and then the temperature is raised to 450° C. at a heating rate of 2° C. / min, and calcined for 2 hours to obtain a BiVO4 film, wherein the vanadium precursor solution is a dimethyl sulfoxide solution containing 0.2 mol / L acetylacetonatovanadium;
[0048] The step of immersing the BiVO4 film in a sodium hydroxide solution to obtain a BiVO4 photoanode specifically comprises:
[0049] The BiVO4 film was immersed in a 1 mol / L sodium hydroxide solution for 35 min to obtain a BiVO4 photoanode.
[0050] Based on the same inventive concept, the present invention provides a composite photoanode for photoelectrocatalytic hydrogen production, and the composite photoanode is prepared by the above-mentioned method for preparing a composite photoanode for photoelectrocatalytic hydrogen production.
[0051] Based on the same inventive concept, the present invention provides a composite photoanode for photoelectrocatalytic hydrogen production, the composite photoanode comprising a BiVO4 photoanode, a FeMOFs layer with a thickness of 0.8 to 1.5 nm loaded on the surface of the BiVO4 layer of the BiVO4 photoanode, and a Co4(μ3-O)4X layer with a thickness of 0.2 to 0.5 nm loaded on the surface of the FeMOFs layer.
[0052] Based on the same inventive concept, the present invention provides an application of a composite photoanode for photoelectrocatalytic hydrogen production in photoelectrocatalytic water decomposition.
[0053] Based on the same inventive concept, the present invention provides an application of a composite photoanode for photoelectrocatalytic hydrogen production in photoelectrocatalytic hydrogen production.
[0054] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0055] 1. The present invention provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production. FeMOFs with the properties of a co-catalyst and a passivation layer are loaded on a BiVO4 film by a hydrothermal method. On the one hand, it can provide active sites for the oxygen evolution reaction, and on the other hand, it can inhibit the V 5+ In addition, the Co4(μ3-O)4X molecular catalyst was further introduced on the BiVO4 / FeMOFs layer by the impregnation method, which formed a Co-Fe dual catalytic site with FeMOFs. The [Co4(μ3-O)4] 4+ Its special tetramer-like cubic core structure can provide more OER reaction points, and can interact with the active sites on BiVO4 / FeMOF, modify the catalytic local environment of BiVO4 / FeMOFs at the molecular level, reduce the recombination of carriers and quickly promote the extraction of holes to the surface to participate in the surface water oxidation process, accelerate the oxygen evolution reaction, and make the composite photoanode have efficient and stable PEC water oxidation performance. The present invention utilizes a combination of hydrothermal method and impregnation method to synthesize the composite photoanode. The synthesis method is simple and clear, easy to operate, and the required materials are widely available. It is an economical, green and environmentally friendly photoanode preparation method. The prepared composite photoanode can achieve relatively excellent photoelectric conversion efficiency in photoelectric water decomposition, and can be efficiently used in photoelectrochemical water decomposition.
[0056] 2. The present invention discloses a composite photoanode for photoelectrocatalytic hydrogen production. MOF materials and molecular catalyst Co4(μ3-O)4X are simultaneously introduced into the BiVO4 film. FeMOFs provide anchoring sites for Co4(μ3-O)4X and form Co-Fe dual catalytic sites with Co4(μ3-O)4X. The two together provide a large number of active sites for the oxygen evolution reaction (OER). As an oxygen evolution co-catalyst (WOC, i.e., FeMOFs@Co4(μ3-O)4X), it improves the h+ transfer and also acts as a passivation layer to minimize V 5+ The dissolution of CoMC enhances the PEC activity and stability of BiVO4 to a certain extent. CoMC is anchored on the Fe metal site of FeMOFs material and coupled with FeMOFs material, which improves the selectivity of water oxidation process, reduces the limitation of water oxidation kinetics, reduces charge recombination and promotes the extraction of holes to the surface, promotes the formation of OO bonds, accelerates the oxygen evolution reaction, and significantly improves the stability and PEC performance of the composite photoanode. According to tests, the photocurrent density of the composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X of the present invention is more than 3.5 times that of the pure BiVO4 electrode, and the PEC performance is greatly enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0058] Figure 1 This is a scanning electron microscope image of the BiVO4 / FeMOFs@Co4(μ3-O)4X-ray anode prepared in Example 1 of the present invention.
[0059] Figure 2 This is a transmission electron microscopy image of the BiVO4 / FeMOFs@Co4(μ3-O)4X-ray anode prepared in Example 1 of the present invention.
[0060] Figure 3 This is the XRD spectrum of the BiVO4 / FeMOFs@Co4(μ3-O)4X-ray anode prepared in Example 1 of the present invention.
[0061] Figure 4 This is the XPS spectrum of the BiVO4 / FeMOFs@Co4(μ3-O)4X-photoanode prepared in Example 1 of the present invention.
[0062] Figure 5This is a linear sweep voltammetric curve of the BiVO4 / FeMOFs@Co4(μ3-O)4X-photoanode prepared in Example 1 and Examples 5-6 of the present invention.
[0063] Figure 6 This is the linear sweep voltammetry curve of the BiVO4 / FeMOFs@Co4(μ3-O)4X-ray photoanode prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0064] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0065] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.
[0066] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0067] The technical principle of the present invention is as follows:
[0068] The present invention aims at the BiVO4 photoanode carriers are easy to recombine, the water oxidation kinetics is slow, and V 5+ In order to solve the problems of poor stability caused by easy leaching, a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production is proposed. FeMOFs with the properties of co-catalyst and passivation layer are loaded on BiVO4 film by hydrothermal method, which can provide active sites for oxygen evolution reaction on the one hand, and inhibit V 5+ In addition, the Co4(μ3-O)4X molecular catalyst was further introduced on the BiVO4 / FeMOFs layer by the impregnation method, which formed a Co-Fe dual catalytic site with FeMOFs. The [Co4(μ3-O)4] 4+ The cubic structure can interact with the active sites on BiVO4 / FeMOF, modifying the catalytic local environment of BiVO4 / FeMOFs at the molecular level, reducing the recombination of carriers and quickly promoting the extraction of holes to the surface to participate in the surface water oxidation process. Therefore, the prepared composite photoanode has efficient and stable PEC water oxidation performance.
[0069] The present invention provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production, comprising:
[0070] S1. Dissolving FeCl3 and H2ATA together in a DMF solution to obtain a mixed solution;
[0071] S2. placing the BiVO4 photoanode in the mixed solution for hydrothermal reaction to obtain a BiVO4 / FeMOFs photoanode;
[0072] S3. Co(NO3)2 and CH3CO2Na are dissolved in an organic solvent, and when heated to a specified temperature, a pyridine solution is added, followed by a hydrogen peroxide solution, and the reaction is stirred at reflux temperature until the color of the mixture changes from purple to dark green to obtain Co4(μ3-O)4X;
[0073] S4. Immerse the BiVO4 / FeMOFs photoanode in the aqueous solution of Co4(μ3-O)4X, then take it out and dry it to obtain a composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X.
[0074] In step S1:
[0075] The molar ratio of FeCl3 to H2ATA in the mixed solution is (1-3):4;
[0076] The molar concentration of FeCl3 in the mixed solution is 0.003-0.005 mol / L;
[0077] The DMF solution is prepared by mixing DMF and water in a volume ratio of 1:1.
[0078] In the present invention, the molar ratio of FeCl3 and H2ATA is (1-3):4. FeCl3 provides loose trivalent iron ions to fully contact with the organic ligands in H2ATA and couple with each other, which is beneficial to the formation of FeMOFs. If it is lower or higher than this ratio range, it is easy to cause insufficient ligand contact, resulting in poor crystallinity of FeMOFs.
[0079] In the present invention, the molar concentration of FeCl3 in the mixed solution is 0.003-0.005 mol / L, which can make Fe 3+ In the appropriate concentration range, it can fully react with other substances to form FeMOFs. Concentrations below or above this range are likely to cause the conductivity of FeMOFs to deteriorate, making it difficult to form Fe-O clusters, and affecting the light absorption of the photoanode. Among them, the DMF in the DMF solution can be used as a high-temperature solvent to reduce the temperature during the synthesis of FeMOFs, accelerate the concentration of water and nitrogen, and promote the formation of the FeMOFs crystal structure.
[0080] Step S2 specifically includes:
[0081] The BiVO4 photoanode is placed in the mixed solution, and subjected to a hydrothermal reaction at 90-120° C. for 18-24 hours. After the hydrothermal reaction is completed, the photoanode is washed and dried to obtain a BiVO4 / FeMOFs photoanode.
[0082] In the present invention, the hydrothermal reaction temperature is 90-120° C., which provides good conditions for the synthesis of FeMOFs and promotes the crystallization process of MOFs. If the temperature is lower or higher than this range, it will affect the crystallization process of MOFs, resulting in clusters of MOFs or poor crystallinity, presenting a powder state.
[0083] Step S3 specifically includes:
[0084] Dissolve Co(NO3)2 and CH3CO2Na in methanol, add pyridine solution when heated to 90±5℃, then slowly add hydrogen peroxide solution, stir and react at 90±5℃ for 4-5h until the color of the mixture changes from purple to dark green, and obtain a mixture containing Co4(μ3-O)4X;
[0085] The Co4(μ3-O)4X-containing mixture is stored at room temperature for 3 to 5 days to obtain Co4(μ3-O)4X crystals, which are then crushed to obtain powdered Co4(μ3-O)4X.
[0086] In the present invention, since the Co4(μ3-O)4X mixture is a solution at the end of the reaction, it is stored at room temperature for 3 to 5 days. The purpose is to volatilize and crystallize the obtained solution for 3 to 5 days, and finally grind the crystals into powder.
[0087] In the present invention, after the pyridine solution is added, pyridine can form a coordination bond with the complex of the Co ion, enhance the electrophilicity of the reactant, and promote the generation of the substance. After the addition of hydrogen peroxide, the reaction and the generation of the Co complex are further accelerated. The reaction temperature is 90±5° C., which is the reflux temperature and can minimize the loss of the substance. If the temperature is lower than this temperature, the substance will crystallize and the reaction will be prevented. If the temperature is higher than this temperature, a large amount of product will be lost.
[0088] In step S3:
[0089] The molar ratio of the Co(NO3)2 and the CH3CO2Na is (1-2):(2-4);
[0090] The molar ratio of the Co(NO3)2 to the pyridine in the pyridine solution is (8-12):1;
[0091] The molar ratio of the Co(NO3)2 to the hydrogen peroxide in the hydrogen peroxide solution is 1:(6-10).
[0092] In the present invention, the molar ratio of Co(NO3)2 and CH3CO2Na is (1-2):(2-4), so that the reaction proceeds fully and provides cobalt ligands for the complex.
[0093] Step S4 specifically includes:
[0094] The BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X for 5 to 60 minutes, and then taken out and dried at room temperature to obtain a composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X;
[0095] Wherein, in the aqueous solution of Co4(μ3-O)4X, the concentration of Co4(μ3-O)4X is 0.5-5 mg / mL.
[0096] In the present invention, the concentration of Co4(μ3-O)4X in the aqueous solution of Co4(μ3-O)4X is 0.5-5 mg / mL, which can further improve the photocurrent density of the BiVO4 / FeMOFs photoanode. Co4(μ3-O)4X can interact better with FeMOFs. If the concentration is lower than this range, it is difficult to load Co4(μ3-O)4X onto the BiVO4 / FeMOFs photoanode. If the concentration is too high, Co4(μ3-O)4X will cover the catalytic sites (OER sites) of the BiVO4 / FeMOFs photoanode, thereby reducing the photocurrent density of BiVO4 / FeMOFs@Co4(μ3-O)4X.
[0097] Specifically, the present invention provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production, comprising:
[0098] 1. Hydrothermal synthesis of BiVO4 / FeMOFs photoanode:
[0099] Take 0.02-0.06g FeCl3·6H2O, add 0.03-0.08g H2ATA, add to 20-30mL DMF solution, stir for 20-30min to obtain a mixed solution; then add the BiVO4 photoanode and the mixed solution into a reactor, hydroheat at 90-120°C for 18-24h, after the reaction is completed, take out the FTO glass sheet, rinse it with DMF and deionized water several times, put it into a vacuum oven and dry it for 2-3h, and then take it out to obtain the BiVO4 / FeMOFs photoanode.
[0100] 2. Synthesis of Co4(μ3-O)4X powder:
[0101] Add 10-20 mmol Co(NO3)2·6H2O and 20-40 mmol CH3CO2Na to 30-60 mL methanol, heat while stirring, add 0.05-0.1 mL pyridine solution when the specified temperature reaches 90±5°C, and continue stirring to form a reaction mixture; then slowly add 5-10 mL hydrogen peroxide solution to the reaction mixture, and continue stirring at a reflux temperature of 90±5°C for 4-5 hours; when the color of the mixture changes from purple to dark green, transfer the concentrated reaction mixture from the flask to a beaker, and store it at room temperature for 3-5 days to obtain a dark green Co4(μ3-O)4X powder.
[0102] 3. Obtain BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode by impregnation method:
[0103] The BiVO4 / FeMOFs photoanode was immersed in a Co4(μ3-O)4X solution with a concentration of 0.5-5 mg / mL for 5-60 min, and the electrode sheet was dried at room temperature to obtain a BiVO4 / FeMOFs@Co4(μ3-O)4X photoanode.
[0104] The following will describe in detail a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production and a composite photoanode of the present application in combination with examples and experimental data.
[0105] Example 1
[0106] The present embodiment provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production, comprising the following steps:
[0107] (1) Synthesis of BiVO4 photoanode by electrodeposition-calcination method:
[0108] The synthesis of BiVO4 photoanode is divided into two steps. The first step is to prepare BiOI by electrodeposition. This process is carried out under a three-electrode system. The second step is to calcine and then immerse in a NaOH solution to obtain a BiVO4 photoanode. In the present invention, the working electrode uses FTO glass produced by Wuhan Jingge, the reference electrode is saturated Ag / AgCl, and the counter electrode uses a platinum electrode with good conductivity and stability.
[0109] Specifically, 0.4M (3.32g) of KI was added to 50mL of deionized water, fully dissolved in the ultrasonic process to obtain a KI solution, and then 0.04M (0.9701g) of BiNO3·5H2O was added to the KI solution, and 20 microliters of concentrated nitric acid solution was added during stirring to adjust the pH to 1.7 to obtain a solution A. Then 0.497g of p-benzoquinone was added to a beaker containing 20mL of anhydrous ethanol to obtain a solution B. Finally, the prepared A and B solutions were mixed and vigorously stirred for 8 minutes to fully mix them to obtain a precursor electrolyte. Electrodeposition was deposited at a constant potential of -0.1V Ag / AgCl, and the deposition time was 180s. After the program was terminated, it was slowly rinsed with deionized water several times to remove other impurities on the surface of the BiOI electrode, and finally a dark yellow electrode sheet was obtained. Next is the calcination process. First, dissolve acetylacetonato vanadium (0.106g) in DMSO solution. Take 2mL of DMSO solution here to obtain a vanadium precursor solution. Drop the prepared vanadium precursor solution onto the surface of the deposited electrode sheet. In this process, select an excess of 150μL solution, and then put it into a muffle furnace and calcine it at 450℃ for 2 hours. During this process, ensure that the temperature in the furnace rises uniformly by 2℃ per minute. After the reaction is completed, wait for the furnace to cool down before taking out the electrode. Then, soak the calcined electrode in 1M NaOH solution for 35min. The main purpose is to remove vanadium pentoxide on the surface of BiVO4. Finally, rinse the electrode surface with deionized water several times and dry it at room temperature to obtain a BiVO4 photoanode.
[0110] (2) Hydrothermal synthesis of BiVO4 / FeMOFs:
[0111] Take 0.027g FeCl3·6H2O, add 0.0362g H2ATA thereto, then add 12mL ultrapure water and 12mL DMF solution, stir for 30min to fully mix them to obtain a mixed solution; add the prepared BiVO4 photoanode and the mixed solution into a 10mL reactor, hydroheat at 90°C for 20h. After the reaction is completed, take out the FTO glass sheet, rinse it with DMF and deionized water several times, put it in a vacuum oven and dry it for 2h to obtain the BiVO4 / FeMOFs photoanode.
[0112] (3) Synthesis of Co4(μ3-O)4X powder:
[0113] Add 10mmol Co(NO3)2·6H2O and 20mmol CH3CO2Na to 30mL methanol, heat while stirring, add 0.08mL pyridine solution when it reaches 90℃, and continue stirring to form a reaction mixture. Slowly add 5mL hydrogen peroxide to the reaction mixture, and continue stirring at reflux temperature (90℃) for 4 hours. When the color of the mixture changes from purple to dark green, transfer the concentrated reaction mixture from the flask to a beaker and store it at room temperature for 3 days to obtain dark green Co4(μ3-O)4X powder.
[0114] (4) BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode was obtained by impregnation method:
[0115] The BiVO4 / FeMOFs photoanode was immersed in a CoMC solution with a concentration of 1 mg / mL for 20 minutes. The electrode sheet was dried at room temperature to obtain the BiVO4 / FeMOFs@Co4(μ3-O)4X photoanode.
[0116] Example 2
[0117] This embodiment provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production. The difference between this preparation method and embodiment 1 is that the immersion time in step (4) is 10 minutes.
[0118] The details are as follows:
[0119] (1) Same as step (1) of Example 1.
[0120] (2) Same as step (2) in Example 1.
[0121] (3) Same as step (3) of Example 1.
[0122] (4) BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode was obtained by impregnation method:
[0123] The BiVO4 / FeMOFs photoanode was immersed in a CoMC solution with a concentration of 1 mg / mL for 10 minutes. The electrode sheet was dried at room temperature to obtain the BiVO4 / FeMOFs@Co4(μ3-O)4X photoanode.
[0124] Example 3
[0125] This embodiment provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production. The difference between this preparation method and embodiment 1 is that the immersion time in step (4) is 60 minutes.
[0126] The details are as follows:
[0127] (1) Same as step (1) of Example 1.
[0128] (2) Same as step (2) in Example 1.
[0129] (3) Same as step (3) of Example 1.
[0130] (4) BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode was obtained by impregnation method:
[0131] The BiVO4 / FeMOFs photoanode was immersed in a CoMC solution with a concentration of 1 mg / mL for 60 minutes. The electrode sheet was dried at room temperature to obtain the BiVO4 / FeMOFs@Co4(μ3-O)4X photoanode.
[0132] Example 4
[0133] The present embodiment provides a method for preparing a composite photoanode for photoelectrocatalytic hydrogen production, comprising the following steps:
[0134] (1) Same as step (1) of Example 1.
[0135] (2) Same as step (3) in Example 1.
[0136] (3) BiVO4 / Co4(μ3-O)4X composite photoanode was obtained by impregnation method:
[0137] The BiVO4 photoanode was immersed in a CoMC solution with a concentration of 1 mg / mL for 20 minutes, and the electrode sheet was dried at room temperature to obtain a BiVO4 / Co4(μ3-O)4X photoanode.
[0138] Example 5
[0139] In this example, the electrode material prepared in Example 1 was characterized and its performance was tested.
[0140] 1. The BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode prepared in Example 1 was characterized by scanning electron microscopy and transmission electron microscopy. The results are shown in the attached figure. Figure 1-2 shown.
[0141] From the attached Figure 1 It can be seen that BiVO4 / FeMOFs@Co4(μ3-O)4X presents a worm-rod structure with a length of 400-500nm and a width of 150-250nm. The worm-rod shape ensures sufficient specific surface area for PEC reaction and brings a large number of contact sites for photoelectrocatalysis. Figure 2 It can be seen that an ultra-thin FeMOFs@Co4(μ3-O)4X layer with a thickness of 1-2 nm is loaded on the surface, and the ultra-thin layer of co-catalyst is more conducive to the extraction of photogenerated holes.
[0142] 2. The BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode prepared in Example 1 was characterized by X-ray diffractometer and X-ray photoelectron spectrometer. The results are shown in the attached figure. Figure 3-4 shown.
[0143] From the attached Figure 3 It can be seen that the pattern of BiVO4 matches well with the monoclinic BiVO4 card. The sharp and strong peaks indicate that the BiVO4 has high crystallinity. Figure 4 The characteristic peaks of elements such as Fe 2p, Co 2p, N 1s and Na 1s can be seen, indicating the successful loading of FeMOFs and Co4(μ3-O)4X.
[0144] 3. The photoanode materials prepared in Example 1 and Example 2-3 were subjected to linear sweep voltammetry test. The results are shown in the attached figure. Figure 5 shown.
[0145] Attached Figure 5 The figure shows the linear voltammetric curves of the BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode immersed in Co4(μ3-O)4X solution for different time periods. When immersed for 20 min, the BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode exhibited the highest photocurrent density, indicating its excellent PEC performance.
[0146] 3. The photoanode materials prepared in Examples 1 and 4 were subjected to linear sweep voltammetry tests. The results are as follows: Figure 6 shown.
[0147] Attached Figure 6 The linear voltammetric curves of BiVO4, BiVO4 / FeMOFs, BiVO4@Co4(μ3-O)4X and BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanodes show that the photocurrent density of the BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode is the highest, indicating the excellent PEC water oxidation performance of the BiVO4 / FeMOFs@Co4(μ3-O)4X material. The photocurrent density of the BiVO4 / FeMOFs@Co4(μ3-O)4X composite photoanode is more than 3.5 times that of the bismuth vanadate photoanode.
[0148] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.
[0149] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0150] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a composite photoanode for photoelectrocatalytic hydrogen production, characterized in that: The preparation method comprises: Dissolving FeCl3 and H2ATA together in a DMF solution to obtain a mixed solution; Placing the BiVO4 photoanode in the mixed solution for hydrothermal reaction to obtain a BiVO4 / FeMOFs photoanode; Co(NO3)2 and CH3CO2Na are dissolved in an organic solvent, and when heated to a specified temperature, a pyridine solution is added, followed by a hydrogen peroxide solution, and the mixture is stirred at reflux temperature until the color of the mixture changes from purple to dark green, thereby obtaining Co4(μ3-O)4X; The BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X, and then taken out and dried to obtain a composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X.
2. The method for preparing a composite photoanode for photoelectrocatalytic hydrogen production according to claim 1, characterized in that: The method of dissolving FeCl3 and H2ATA in a DMF solution to obtain a mixed solution specifically comprises: Dissolving FeCl3 and H2ATA together in a DMF solution to obtain a mixed solution; Wherein, the molar ratio of FeCl3 and H2ATA in the mixed solution is (1-3):4; The molar concentration of FeCl3 in the mixed solution is 0.003-0.005 mol / L; The DMF solution is prepared by mixing DMF and water in a volume ratio of 1:
1.
3. The method for preparing a composite photoanode for photoelectrocatalytic hydrogen production according to claim 1, characterized in that: The step of placing the BiVO4 photoanode in the mixed solution for hydrothermal reaction to obtain the BiVO4 / FeMOFs photoanode specifically includes: The BiVO4 photoanode is placed in the mixed solution, and subjected to a hydrothermal reaction at 90-120° C. for 18-24 hours. After the hydrothermal reaction is completed, the photoanode is washed and dried to obtain a BiVO4 / FeMOFs photoanode.
4. The method for preparing a composite photoanode for photoelectrocatalytic hydrogen production according to claim 1, characterized in that: The method comprises dissolving Co(NO3)2 and CH3CO2Na in an organic solvent, adding a pyridine solution when heated to a specified temperature, and then adding a hydrogen peroxide solution, and stirring the reaction at a reflux temperature until the color of the mixture changes from purple to dark green to obtain Co4(μ3-O)4X, which specifically comprises: Dissolve Co(NO3)2 and CH3CO2Na in methanol, add pyridine solution when heated to 90±5℃, then slowly add hydrogen peroxide solution, stir and react at 90±5℃ for 4-5h until the color of the mixture changes from purple to dark green, and obtain a mixture containing Co4(μ3-O)4X; The Co4(μ3-O)4X-containing mixture is stored at room temperature for 3 to 5 days to obtain powdered Co4(μ3-O)4X.
5. The method for preparing a composite photoanode for photoelectrocatalytic hydrogen production according to claim 4, characterized in that: The molar ratio of the Co(NO3)2 and the CH3CO2Na is (1-2):(2-4); The molar ratio of the Co(NO3)2 to the pyridine in the pyridine solution is (8-12):1; The molar ratio of the Co(NO3)2 to the hydrogen peroxide in the hydrogen peroxide solution is 1:(6-10).
6. The method for preparing a composite photoanode for photoelectrocatalytic hydrogen production according to claim 1, characterized in that: The BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X, and then taken out and dried to obtain the composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X, which specifically includes: The BiVO4 / FeMOFs photoanode is immersed in the aqueous solution of Co4(μ3-O)4X for 5 to 60 minutes, and then taken out and dried at room temperature to obtain a composite photoanode BiVO4 / FeMOFs@Co4(μ3-O)4X; Wherein, in the aqueous solution of Co4(μ3-O)4X, the concentration of Co4(μ3-O)4X is 0.5-5 mg / mL.
7. A composite photoanode for photoelectrocatalytic hydrogen production, characterized in that: The composite photoanode is prepared by the method for preparing a composite photoanode for photoelectrocatalytic hydrogen production according to any one of claims 1 to 5.
8. A composite photoanode for photoelectrocatalytic hydrogen production, characterized in that: The composite photoanode comprises a BiVO4 photoanode, a FeMOFs layer with a thickness of 0.8 to 1.5 nm is loaded on the surface of the BiVO4 layer of the BiVO4 photoanode, and a Co4(μ3-O)4X layer with a thickness of 0.2 to 0.5 nm is loaded on the surface of the FeMOFs layer.
9. Use of the composite photoanode for photoelectrocatalytic hydrogen production as claimed in claim 7 or 8 in photoelectrocatalytic water decomposition.
10. Use of the composite photoanode for photoelectrocatalytic hydrogen production as claimed in claim 7 or 8 in photoelectrocatalytic hydrogen production.
Citation Information
Patent Citations
Preparation method of ZnO / BiVO<4> heterojunction photoanode composite material for photochemical decomposition of water
CN110373680A
OV-BiVO4 composite photo-anode coated with MOFs, and preparation method and application of OV-BiVO4 composite photo-anode
CN110983362A
Preparation method and application of BiVO4 / Ni MOF / Co-Pi composite photo-anode
CN115747829A