Preparation method of cyanide-free zinc plating additive and cyanide-free zinc plating additive

Through the preparation method of cyanide galvanizing additives, the problems of low current efficiency, toxic properties and insufficient performance of galvanized layers in the traditional cyanide galvanizing process are solved, and efficient and safe preparation of galvanized layers is achieved, with good flatness , gloss and corrosion resistance.

CN119061442APending Publication Date: 2024-12-03FOSHAN RENCHANG TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411028259.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The traditional cyanide galvanizing process has problems such as low current efficiency, toxic properties, poor dispersion ability of the galvanized layer, poor gloss and insufficient corrosion resistance.

Method used

The preparation method of cyanide-free galvanized additives is adopted. By mixing auxiliary additives, complexing agents, leveling agents and water, adding brighteners, wetting agents and antioxidants, adjusting the pH value to form an efficient cyanide-free galvanized additive. It is used in electroplating processes to improve the flatness, gloss and corrosion resistance of the galvanized layer.

Benefits of technology

The dispersion ability of the galvanized plating solution is significantly improved, the galvanized layer is flat, has good gloss, and has improved corrosion resistance, meeting industrial requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The preparation method comprises the following steps that S1, a mixture containing an auxiliary additive, a complexing agent, a leveling agent and water is stirred I, and a first mixed solution is obtained; and S2, a brightener, a wetting agent and an antioxidant are added into the first mixed solution to be mixed, stirring II is conducted, the pH is adjusted, and the cyanide-free zinc plating additive is obtained. According to the preparation method of the cyanide-free zinc plating additive, the efficient cyanide-free zinc plating additive is prepared, after the cyanide-free zinc plating additive is added and used, the dispersing capacity and other performance of a zinc plating solution are well improved, and a zinc plating layer is flat, good in glossiness and good in corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a preparation method of a cyanide-free zinc plating additive and a cyanide-free zinc plating additive, belonging to the technical field of additives for electroplating. Background Art

[0002] Electroplating is the process of plating a thin layer of other metals or alloys on certain metal surfaces using the principle of electrolysis. It is a process that uses electrolysis to adhere a layer of metal film to the surface of metal or other material parts, thereby preventing metal oxidation (such as rust), improving wear resistance, conductivity, reflectivity, corrosion resistance (copper sulfate, etc.) and enhancing aesthetics.

[0003] Traditional alkaline zinc plating is mainly based on cyanide zinc plating. The cyanide electroplating process has always occupied an important position in the alkaline zinc plating process due to its wide process range and high impurity tolerance, especially in national defense and military industrial products. In the cyanide zinc plating process, cyanide is very critical. Zinc ions and cyanide form cyano-zinc complex ions. The presence of complex ions inhibits the discharge of zinc ions at the cathode and improves cathode polarization, thereby playing a role in refining crystals. At the same time, because cyanide can improve cathode polarization, it affects the primary current distribution and secondary current distribution on the cathode surface, making it more uniform, and correspondingly improves the dispersion ability.

[0004] However, the current efficiency of cyanide solution is relatively low, and cyanide solution can react with CO2 in the air to produce cyanide carbonation, while producing toxic HCN which is not stable enough. At the same time, cyanide is a highly toxic drug, which may cause great safety hazards to the environment and personnel during production, transportation and use.

[0005] The galvanizing additives currently used still have the following problems: poor dispersibility of the galvanizing solution, uneven galvanized layer, poor gloss, and poor corrosion resistance. Summary of the invention

[0006] In view of the problems existing in the above-mentioned prior art, the present application proposes a method for preparing a cyanide-free zinc plating additive, which can effectively solve the above-mentioned problems.

[0007] According to one aspect of the present application, a method for preparing a cyanide-free zinc plating additive is provided, the preparation method comprising the following steps:

[0008] S1: stirring a mixture containing auxiliary additives, complexing agents, leveling agents and water for I to obtain a first mixed solution;

[0009] S2: adding a brightener, a wetting agent and an antioxidant into the first mixed solution, stirring II, and adjusting the pH to obtain the cyanide-free zinc plating additive.

[0010] Optionally, in step S2, the brightener is selected from at least one of benzyl acetone, benzylamine, acetylene alcohol compounds, benzyl chloride, thiourea and its derivatives, and p-methoxybenzaldehyde.

[0011] Optionally, the brightener is p-methoxybenzaldehyde.

[0012] Optionally, the dosage ratio of the brightener to the first mixed liquid is (0.5-3):(25-450).

[0013] Optionally, in step S2, the wetting agent is selected from sodium alkyl sulfonate and / or sodium alkylbenzene sulfonate.

[0014] Optionally, the antioxidant is selected from ascorbic acid and / or sodium metabisulfite.

[0015] Optionally, the dosage ratio of the wetting agent to the antioxidant is (2-5): (0.3-5).

[0016] Optionally, the usage ratio of the brightener to the wetting agent is (0.5-3):(2-6).

[0017] Optionally, in step S1, the auxiliary additive is selected from at least one of aluminum salt, zinc salt, potassium salt and ammonium salt.

[0018] Optionally, the aluminum salt is selected from at least one of aluminum sulfate, aluminum chloride and aluminum nitrate.

[0019] Optionally, the zinc salt is selected from at least one of zinc chloride, zinc sulfate and zinc nitrate.

[0020] Optionally, the potassium salt is selected from at least one of potassium chloride, potassium nitrate and potassium nitrate.

[0021] Optionally, the ammonium salt is selected from at least one of ammonium nitrate, ammonium sulfate and ammonium chloride.

[0022] Optionally, in step S1, the complexing agent is selected from at least one of ethylenediaminetetraacetic acid, triethanolamine, sodium citrate and glycine.

[0023] Optionally, the leveling agent is selected from at least one of polyethylene glycol, polyacrylamide, and sodium N,N-dimethyldithiocarbamate.

[0024] Optionally, in step S1, the dosage ratio of the auxiliary additive to the complexing agent is (25-500): (2-3).

[0025] Optionally, the dosage ratio of the complexing agent to the leveling agent is (2-3): (0.1-1).

[0026] Optionally, the auxiliary additive is used in the first mixed liquid in an amount of 5% to 30%.

[0027] Optionally, the dosage ratio of the auxiliary additive in the first mixed liquid is independently selected from any value of 5%, 10%, 15%, 20%, 25%, 30% or a range between any two of the above.

[0028] Optionally, in step S2, the pH regulator is selected from at least one of boric acid, acetic acid, sodium hydroxide and potassium hydroxide.

[0029] Optionally, the pH value of the cyanide-free zinc plating additive is 4-6.

[0030] Optionally, the pH value of the cyanide-free zinc plating additive is independently selected from any value of 4, 4.5, 5, 5.5, 6, or a range between any two of the above values.

[0031] Optionally, in step S1, the temperature of the stirring I is 20 to 50° C., the rotation speed of the stirring I is 150 to 500 r / min, and the time of the stirring I is 2 to 6 h.

[0032] Optionally, in step S1, the stirring temperature I is independently selected from any value of 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or a range between any two of the above values.

[0033] Optionally, in step S1, the rotation speed of the stirring I is independently selected from any value of 150r / min, 200r / min, 250r / min, 300r / min, 350r / min, 400r / min, 450r / min, 500r / min or a range between any two of the above.

[0034] Optionally, in step S1, the stirring time I is independently selected from any value among 2h, 3h, 4h, 5h, 6h or a range between any two of the above.

[0035] Optionally, in step S2, the temperature of stirring II is 30-80° C., the rotation speed of stirring II is 100-600 r / min, and the time of stirring II is 2-8 h.

[0036] Optionally, in step S2, the temperature of the stirring II is independently selected from any value of 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 70°C, 80°C or a range between any two of the above values.

[0037] Optionally, in step S2, the rotation speed of the stirring II is independently selected from any value of 100r / min, 150r / min, 200r / min, 250r / min, 300r / min, 350r / min, 400r / min, 450r / min, 500r / min, 600r / min or a range between any two of the above.

[0038] Optionally, in step S2, the stirring time II is independently selected from any value among 2h, 3h, 4h, 5h, 6h, 8h or a range between any two of the above.

[0039] As an optional implementation method, the present application is implemented through the following technical solutions:

[0040] In the present application, the preparation method of the cyanide-free zinc plating additive comprises the following steps:

[0041] (1) dissolving zinc chloride in deionized water, adding potassium chloride and boric acid, fully dissolving and mixing, to obtain a first mixed solution;

[0042] (2) adding a complexing agent and a leveling agent to the first mixed solution and mixing and stirring to obtain a second mixed solution;

[0043] (3) adding the brightener, wetting agent and antioxidant into the second mixed solution, stirring and mixing evenly, adjusting the pH value between 4 and 6, and obtaining the cyanide-free zinc plating additive.

[0044] The beneficial effects of this application include:

[0045] The preparation method of the cyanide-free zinc plating additive disclosed in the present application prepares a highly efficient cyanide-free zinc plating additive, which not only greatly improves the dispersibility and other properties of the zinc plating solution after being added, but also makes the zinc plating layer smooth, glossy and corrosion-resistant. DETAILED DESCRIPTION

[0046] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0047] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0048] Unless otherwise specified, the instruments used in this application are conventional existing instruments and equipment and operating conditions.

[0049] Example 1

[0050] (1) Weighing 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water into a container, stirring at 150 r / min and 20° C. for 2 h on a magnetic stirrer to obtain a first mixed solution that is uniformly mixed;

[0051] (2) Add 0.5 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant to the first mixed solution, and then add 485.1 g of water to mix, stir for 2 h at 30° C. with a magnetic stirrer at 100 r / min, and adjust the pH value to 4 with boric acid to obtain a cyanide-free zinc plating additive, and heat at 25° C. and a current density of 2 A / dm 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0052] Example 2

[0053] (1) Weigh 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water, add them into a container, stir them at 500 r / min and 50° C. on a magnetic stirrer for 6 h to obtain a first mixed solution that is uniformly mixed;

[0054] (2) Add 0.5 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant to the first mixed solution, and then add 485.1 g of water to mix, stir at 600 r / min and 80° C. for 8 h on a magnetic stirrer, adjust the pH value to 6 with boric acid, and obtain a cyanide-free zinc plating additive. 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0055] Example 3

[0056] (1) Weigh 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water, add them into a container, and stir them at 300 r / min and 40° C. on a magnetic stirrer for 3 h to obtain a first mixed solution that is uniformly mixed;

[0057] (2) Add 0.5 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant to the first mixed solution, and then add 485.1 g of water to mix, stir for 5 h at 400 r / min and 50° C. with a magnetic stirrer, adjust the pH value to 5 with boric acid, and obtain a cyanide-free zinc plating additive. 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0058] Example 4

[0059] (1) Weigh 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water, add them into a container, and stir them at 300 r / min and 40° C. on a magnetic stirrer for 3 h to obtain a first mixed solution that is uniformly mixed;

[0060] (2) Add 1 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant to the first mixed solution, and then add 485.1 g of water to mix, stir for 5 h at 400 r / min and 50° C. with a magnetic stirrer, adjust the pH value to 5 with boric acid, and obtain a cyanide-free zinc plating additive. 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0061] Example 5

[0062] (1) Weigh 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water, add them into a container, and stir them at 300 r / min and 40° C. on a magnetic stirrer for 3 h to obtain a first mixed solution that is uniformly mixed;

[0063] (2) Add 2 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant to the first mixed solution, add 485.1 g of water again, stir for 5 h at 400 r / min and 50° C. with a magnetic stirrer, adjust the pH value to 5 with boric acid, and obtain a cyanide-free zinc plating additive. 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0064] Example 6

[0065] (1) Weigh 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water, add them into a container, and stir them at 300 r / min and 40° C. on a magnetic stirrer for 3 h to obtain a first mixed solution that is uniformly mixed;

[0066] (2) Add 3 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant to the first mixed solution, and then add 485.1 g of water to mix, stir for 5 h at 400 r / min and 50° C. with a magnetic stirrer, adjust the pH value to 5 with boric acid, and obtain a cyanide-free zinc plating additive. 2 Electroplating is carried out under the condition of high temperature to obtain a bright and uniform zinc plating layer.

[0067] Comparative Example 1

[0068] (1) Weigh 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, 0.5 g of p-methoxybenzaldehyde brightener, and 400 g of water, add them into a container, stir them at 150 r / min and 20° C. on a magnetic stirrer for 2 h to obtain a first mixed solution that is uniformly mixed;

[0069] (2) Add 2 g of sodium alkyl sulfonate wetting agent, 0.3 g of ascorbic acid antioxidant to the first mixed solution, add 485.1 g of water again, stir for 2 h at 30 ° C with a magnetic stirrer at 100 r / min, adjust the pH value to 4 with boric acid, and obtain a cyanide-free zinc plating additive. 2 If electroplating is carried out under this condition, a bright and uniform zinc plating layer cannot be obtained.

[0070] Comparative Example 2

[0071] (1) Weigh 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, 1 g of p-methoxybenzaldehyde brightener, and 400 g of water, add them into a container, stir them at 150 r / min and 20° C. on a magnetic stirrer for 2 h to obtain a first mixed solution that is uniformly mixed;

[0072] (2) Add 2 g of sodium alkyl sulfonate wetting agent, 0.3 g of ascorbic acid antioxidant to the first mixed solution, add 485.1 g of water again, stir for 2 h at 30 ° C with a magnetic stirrer at 100 r / min, adjust the pH value to 4 with boric acid, and obtain a cyanide-free zinc plating additive. 2 If electroplating is carried out under this condition, a bright and uniform zinc plating layer cannot be obtained.

[0073] Test Example 1

[0074] 1. The plated parts with an average coating thickness of 25 μm were subjected to thermal shock test according to JB-2111-77 standard to detect the bonding strength of the galvanized layer. The specific experimental results are shown in Table 1.

[0075] 2. Take the same workpiece and galvanize it according to the same process. The coating thickness is 10-15μm. After passivation with trivalent chromium passivation solution, place it for 24 hours. Perform a neutral salt spray test for 72 hours according to ISO9227-2006 standard to detect the corrosion of the galvanized layer. The specific experimental results are shown in Table 1.

[0076] Table 1

[0077] Example Binding force Corrosive Example 1 excellent excellent Example 2 excellent excellent Example 3 excellent good Example 4 good excellent Example 5 excellent good Example 6 excellent excellent Comparative Example 1 Difference Difference Comparative Example 2 Difference Difference

[0078] As can be seen from Table 1, the cyanide-free zinc plating additive prepared by the preparation method of the cyanide-free zinc plating additive disclosed in the present application is electroplated on a workpiece for performance testing. The zinc-plated layers in Examples 1 to 6 all have excellent bonding strength and corrosion resistance, and the zinc-plated layers have no appearance changes, and can meet industry requirements. The zinc-plated layers in Comparative Examples 1 and 2 have poor bonding strength, are easily corroded, and have spots on the appearance of the coating, which cannot meet industry requirements.

[0079] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a cyanide-free zinc plating additive, characterized in that: The preparation method comprises the following steps: S1: stirring a mixture containing auxiliary additives, complexing agents, leveling agents and water for I to obtain a first mixed solution; S2: adding a brightener, a wetting agent and an antioxidant into the first mixed solution, stirring II, and adjusting the pH to obtain the cyanide-free zinc plating additive.

2. The preparation method according to claim 1, characterized in that: In step S2, the brightener is selected from at least one of benzyl acetone, benzylamine, acetylene alcohol compounds, benzyl chloride, thiourea and its derivatives, and p-methoxybenzaldehyde; Preferably, the dosage ratio of the brightener to the first mixed solution is (0.5-3):(25-450).

3. The preparation method according to claim 1, characterized in that: In the step S2, the wetting agent is selected from sodium alkyl sulfonate and / or sodium alkylbenzene sulfonate; Preferably, the antioxidant is selected from ascorbic acid and / or sodium metabisulfite; Preferably, the dosage ratio of the wetting agent to the antioxidant is (2-5): (0.3-5); Preferably, the usage ratio of the brightener to the wetting agent is (0.5-3):(2-6).

4. The preparation method according to claim 1, characterized in that: In step S1, the auxiliary additive is selected from at least one of aluminum salt, zinc salt, potassium salt and ammonium salt; Preferably, the aluminum salt is selected from at least one of aluminum sulfate, aluminum chloride and aluminum nitrate; Preferably, the zinc salt is selected from at least one of zinc chloride, zinc sulfate and zinc nitrate; Preferably, the potassium salt is selected from at least one of potassium chloride, potassium nitrate and potassium nitrate; Preferably, the ammonium salt is selected from at least one of ammonium nitrate, ammonium sulfate and ammonium chloride.

5. The preparation method according to claim 1, characterized in that: In step S1, the complexing agent is selected from at least one of ethylenediaminetetraacetic acid, triethanolamine, sodium citrate, and glycine; Preferably, the leveling agent is selected from at least one of polyethylene glycol, polyacrylamide, and sodium N,N-dimethyldithiocarbamate.

6. The preparation method according to claim 1, characterized in that: In the step S1, the dosage ratio of the auxiliary additive to the complexing agent is (25-500): (2-3); Preferably, the dosage ratio of the complexing agent to the leveling agent is (2-3): (0.1-1); Preferably, the mass ratio of the auxiliary additive in the first mixed liquid is 5% to 30%.

7. The preparation method according to claim 1, characterized in that: In step S2, the pH adjusting agent is selected from at least one of boric acid, acetic acid, sodium hydroxide and potassium hydroxide.

8. The preparation method according to claim 1, characterized in that: The pH value of the cyanide-free zinc plating additive is 4-6.

9. The preparation method according to claim 1, characterized in that: In the step S1, the temperature of the stirring I is 20 to 50° C., the speed of the stirring I is 150 to 500 r / min, and the time of the stirring I is 2 to 6 h; Preferably, in step S2, the temperature of stirring II is 30-80° C., the rotation speed of stirring II is 100-600 r / min, and the time of stirring II is 2-8 h.

10. The cyanide-free zinc plating additive prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Acid zinc plating baths and methods for electrodepositing bright zinc deposits