Epitaxial wafer and preparation method and application thereof
By optimizing the buffer layer process to form a stable composite layer, the problems of large surface roughness and high cost of GaN epitaxial layer are solved, and the growth of high-quality ultra-thin epitaxial layer is achieved, thereby reducing production costs.
Patent Information
- Application Number
- CN202310648885.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
During the epitaxial growth process of GaN materials, dislocation and warping are caused by differences in lattice constant and thermal expansion coefficient, resulting in large surface roughness of the epitaxial layer. The prior art requires the growth of thicker epitaxial layers to improve crystal quality, which increases the cost.
By optimizing the preparation process of the buffer layer, a composite layer with good stability, consistent phase and uniform distribution is formed, providing a growth template for subsequent growth of roughened layer and epitaxial layer, achieving high-quality ultra-thin epitaxial layer growth and reducing costs.
The problem of high surface roughness of the epitaxial layer is overcome, and high-quality ultra-thin epitaxial layer growth is achieved, which reduces production costs and improves the cost competitiveness of epitaxial products.
Smart Images

Figure CN119061470A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to an epitaxial wafer and a preparation method and application thereof. Background Art
[0002] GaN-based semiconductor materials have the characteristics of high bandgap, high critical breakdown electric field, high carrier saturation migration velocity, high thermal conductivity and direct bandgap, and have great application prospects in the fields of high-temperature, high-frequency, high-power microelectronic devices and high-performance optoelectronic devices. Due to the lack of homogeneous substrates, GaN materials are usually grown epitaxially on heterogeneous substrates. Due to the large differences in lattice constants and thermal expansion coefficients between GaN materials and substrates, a large number of dislocations will be generated during the epitaxial growth process, and the epitaxial film will also warp and even crack. In addition, the realization of nitride heteroepitaxial wafers based on existing technologies can maximize benefits, which is of great significance to the sustainable development of enterprises.
[0003] However, based on the mechanism that the out-of-plane tilt angle and in-plane twist angle of the epitaxial layer grains decrease with the increase of film thickness, the crystal quality of the epitaxial layer will become higher and higher with the increase of thickness. Thick epitaxial layers require longer growth time and more raw material consumption. Currently, it is usually necessary to grow thick nitride epitaxial layers (at least 2μm) to meet the crystal quality requirements, which is not conducive to cost reduction.
[0004] Therefore, how to achieve the growth of high-quality ultra-thin epitaxial layers while reducing costs is a technical problem that urgently needs to be solved. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an epitaxial wafer and a preparation method and application thereof. The present invention optimizes the preparation process of the buffer layer to form a composite layer with good stability, consistent phase and uniform distribution, improves the nucleation uniformity of the buffer layer, provides a growth template for the subsequent growth of the roughened layer and the epitaxial layer, and finally obtains a high-quality epitaxial layer with a smooth surface, overcoming the problem of large surface roughness of the thin epitaxial layer grown in the conventional epitaxial growth process; moreover, the present invention does not need to adopt the conventional process to grow a thicker epitaxial layer to improve the crystal quality of the epitaxial layer, and realizes the growth of high-quality ultra-thin epitaxial layers, effectively reducing the cost of epitaxial production and improving the cost competitiveness of epitaxial products.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing an epitaxial wafer, the method comprising the following steps:
[0008] (1) growing a composite layer on a substrate, wherein the composite layer comprises a plurality of stacked buffer layers, the buffer layer comprises a first sub-buffer layer and a second sub-buffer layer which are stacked, the first sub-buffer layer is formed by introducing a first precursor, the second sub-buffer layer is formed by introducing a second precursor and a third precursor, and an introduction flow rate f1 of the first precursor is greater than an introduction flow rate f2 of the second precursor;
[0009] (2) growing a roughened layer on the composite layer;
[0010] (3) Growing an epitaxial layer on the roughened layer.
[0011] The present invention optimizes the preparation process of the buffer layer by controlling the inlet flow rate f1 of the first precursor to be greater than the inlet flow rate f2 of the second precursor, thereby finally forming a composite layer with good stability, consistent phase and uniform distribution, improving the nucleation uniformity of the buffer layer, providing a growth template for the subsequent growth of a roughened layer and an epitaxial layer, and finally obtaining a high-quality epitaxial layer with a smooth surface, thereby overcoming the problem of large surface roughness of a thin epitaxial layer grown in a conventional epitaxial growth process; moreover, the present invention does not need to adopt a conventional process to grow a thicker epitaxial layer to improve the crystal quality of the epitaxial layer, thereby achieving the growth of a high-quality ultra-thin epitaxial layer, effectively reducing the cost of epitaxial production, and improving the cost competitiveness of epitaxial products.
[0012] As a preferred technical solution of the present invention, the step (1) specifically comprises:
[0013] (a) introducing a first precursor to form a first sub-buffer layer on the first growth layer;
[0014] (b) introducing a second precursor and a third precursor to form a second sub-buffer layer on the first sub-buffer layer;
[0015] (c) repeating steps (a) and (b) alternately to obtain the composite layer;
[0016] The first growth layer is the substrate or the second sub-buffer layer formed in the previous step (b).
[0017] It should be noted that in the present invention, when the first step (a) and (b) are performed, the first growth layer is the substrate; starting from the second time, the first growth layer is the second sub-buffer layer grown in the previous time. The "second growth layer" and "third growth layer" described below are the same.
[0018] The present invention finally forms a composite layer with good stability, consistent phase and uniform distribution through the above steps (a)-(c), improves the nucleation uniformity of the composite layer, and also improves the uniformity of the distribution of nucleation centers of the coarsening layer. Otherwise, once the coarsening centers formed subsequently are uneven, it will be difficult to form an epitaxial layer with a complete surface and good flatness.
[0019] As a preferred technical solution of the present invention, in step (1), the first precursor and the second precursor are independently group III A organic source precursors.
[0020] Preferably, the Group III A element in the Group III A organic source precursor includes any one of indium, gallium or aluminum, or a combination of at least two of them.
[0021] Preferably, the Group III A organic source precursor includes a Group III A organic compound, and the Group III A organic compound includes any one of an organic indium compound, an organic gallium compound or an organic aluminum compound, or a combination of at least two of them.
[0022] Preferably, the organic indium compound includes any one of trimethyl indium, triethyl indium or dimethyl ethyl indium, or a combination of at least two thereof.
[0023] Preferably, the organic gallium compound includes any one of trimethyl gallium, triethyl gallium or triisopropyl gallium, or a combination of at least two thereof.
[0024] Preferably, the organoaluminum compound includes any one or a combination of at least two of trimethylaluminum, triethylaluminum, dimethylaluminum alkoxide, dimethylaluminum hydride or an alkanes complex.
[0025] Preferably, the third precursor in step (1) is a group VA source precursor.
[0026] Preferably, the group VA source precursor includes a nitrogen source precursor.
[0027] Preferably, the nitrogen source precursor includes any one of NH3, organic amine compounds or trap compounds, or a combination of at least two of them.
[0028] Preferably, the organic amine compound comprises alkylamine.
[0029] Preferably, the alkylamine comprises tert-butylamine and / or n-propylamine.
[0030] Preferably, the trap compound comprises dimethyl trap.
[0031] As a preferred technical solution of the present invention, in step (a), the flow rate f1 of the first precursor is 5-100sccm, for example, it can be 5sccm, 10sccm, 20sccm, 30sccm, 40sccm, 50sccm, 60sccm, 70sccm, 80sccm, 90sccm or 100sccm, etc.
[0032] In the present invention, a first sub-buffer layer of a specific thickness can be formed on the substrate by introducing a first precursor with a high flow rate.
[0033] Preferably, the time for introducing the first precursor in step (a) is 5-10 s, for example, 5 s, 6 s, 7 s, 8 s, 9 s or 10 s.
[0034] Preferably, the step (b) specifically comprises:
[0035] (b1) introducing a second precursor with a flow rate of f2 and a third precursor with a flow rate of f3 under the first set condition;
[0036] (b2) Under the second setting conditions, a second precursor with a flow rate of f4 and a third precursor with a flow rate of f5 are introduced.
[0037] Preferably, in the first setting condition, the temperature is 500-1000°C, for example, 500°C, 600°C, 700°C, 800°C, 900°C or 1000°C, and the time is 2-5s, for example, 2s, 3s, 4s or 5s.
[0038] Preferably, in the second setting condition, the temperature is 500-1000°C, for example, 500°C, 600°C, 700°C, 800°C, 900°C or 1000°C, and the time is 5-10s, for example, 2s, 3s, 4s or 5s.
[0039] Preferably, in step (b), f2<f4<f1.
[0040] In the present invention, the flow rate of the second precursor in step (b2) is between the flow rate of the first precursor and the flow rate of the second precursor in step (b1), which can effectively avoid the uneven growth of the composite layer caused by f4 being too large, because under relatively low temperature conditions, the migration of group III A atoms is relatively poor, which will cause uneven distribution of group III A elements during the growth of the composite layer.
[0041] In addition, this condition can effectively regulate the growth rate of the composite layer, so that the composite layer grows at a relatively low growth rate, so that the surface of the generated IIIA precursor covering layer (i.e., the first sub-buffer layer grown using a IIIA organic source precursor) is uniformly nucleated, and finally a composite layer with uniform distribution and consistent phase orientation is formed on the substrate.
[0042] Preferably, the f2 in step (b) is 5-100 sccm, for example, it can be 5 sccm, 10 sccm, 20 sccm, 30 sccm, 40 sccm, 50 sccm, 60 sccm, 70 sccm, 80 sccm, 90 sccm or 100 sccm, etc.
[0043] Preferably, the f4 in step (b) is 5-100 sccm, for example, it can be 5 sccm, 10 sccm, 20 sccm, 30 sccm, 40 sccm, 50 sccm, 60 sccm, 70 sccm, 80 sccm, 90 sccm or 100 sccm, etc.
[0044] Preferably, in step (b), f5<f3.
[0045] In the present invention, the flow rate of the third precursor in step (b2) is less than the flow rate of the third precursor in step (b1), which can effectively regulate the growth rate of the composite layer, so that the composite layer grows at a relatively low growth rate, and finally forms a composite layer with uniform distribution of group III A elements on the substrate, thereby improving the stability of the composite layer.
[0046] Preferably, the f3 in step (b) is 20-100 slm, for example, 20 slm, 30 slm, 40 slm, 50 slm, 60 slm, 70 slm, 80 slm, 90 slm or 100 slm, etc.
[0047] Preferably, the f5 in step (b) is 20-100 slm, for example, 20 slm, 30 slm, 40 slm, 50 slm, 60 slm, 70 slm, 80 slm, 90 slm or 100 slm, etc.
[0048] As a preferred technical solution of the present invention, the step (2) specifically comprises:
[0049] (A1) thermally annealing the composite layer;
[0050] (B1) growing a first roughened layer on the second grown layer under a third setting condition;
[0051] (C1) growing a second rough layer on the first rough layer under fourth setting conditions;
[0052] (D1) Repeating steps (B1) to (C1) alternately to obtain the roughened layer described in step (2);
[0053] The second growth layer is the composite layer or the second roughened layer generated in the previous step (C1).
[0054] On the basis of the above-mentioned composite layer, the present invention optimizes the growth process of the roughened layer and adjusts the longitudinal and lateral growth modes of the roughened layer. The longitudinal roughening effect of the roughened layer is enhanced, which can delay the lateral epitaxial growth process of the epitaxial layer, and is beneficial to improving the crystal quality of the epitaxial layer; the lateral distribution of the nucleation center is adjusted, so that the laterally grown roughened layer can be distributed on the substrate between the longitudinal nucleation centers, which can accelerate the merging of subsequent epitaxial layers and improve the surface smoothness of the epitaxial layer, thereby finally obtaining a high-quality epitaxial layer with a smooth surface, overcoming the problem of large surface roughness when growing a thin epitaxial layer in a conventional epitaxial growth process.
[0055] As a preferred technical solution of the present invention, the step (2) specifically comprises:
[0056] (A2) thermally annealing the third growth layer;
[0057] (B2) growing a first roughened layer on the third growth layer under a third setting condition;
[0058] (C2) growing a second rough layer on the first rough layer under fourth setting conditions;
[0059] (D2) Repeating steps (A2) to (C2) alternately to obtain the roughened layer described in step (2);
[0060] The third growth layer is the composite layer or the second roughened layer generated in the previous step (C2).
[0061] The present invention repeats step (A2) during the preparation of the roughened layer in order to thermally anneal the formed roughened layer, thereby decomposing nucleation centers with poor crystal phase consistency and improving the consistency of nucleation centers of the epitaxial layer.
[0062] As a preferred technical solution of the present invention, the temperature of the thermal annealing in step (A2) is 1080-1100°C, for example, it can be 1080°C, 1085°C, 1090°C, 1095°C or 1100°C.
[0063] The present invention performs thermal annealing within the range of 1080-1100° C., which can prompt the composite layer to quickly form three-dimensional nucleation point agglomeration, thereby forming the nucleation center of the epitaxial layer.
[0064] Preferably, the thermal annealing time in step (A2) is 2-5s, for example, 2s, 3s, 4s, 5s, etc.
[0065] Preferably, in the third setting condition of step (B2), the temperature is 1050-1060°C, for example, it can be 1050°C, 1052°C, 1054°C, 1056°C, 1058°C or 1060°C.
[0066] The present invention grows the first roughening layer in the range of 1050-1060° C., so that the roughening layer can grow longitudinally with the nucleation center formed in step (A2), which can improve the three-dimensional growth of the roughening layer, further increase the longitudinal distribution of the nucleation center, and improve the growth quality of the epitaxial layer.
[0067] Preferably, in step (B2), the thickness of the first roughened layer is 10-20 nm, for example, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm or 20 nm.
[0068] Preferably, in the fourth setting condition of step (C2), the temperature is 1060-1080°C, for example, it can be 1060°C, 1065°C, 1070°C, 1075°C or 1080°C.
[0069] The present invention grows the second roughening layer in the range of 1060-1080°C, which promotes the lateral growth of the roughening layer to a certain extent, and adjusts the lateral distribution of the nucleation centers in step (B2), so that the laterally grown roughening layer can be distributed on the substrate between the longitudinal nucleation centers, thereby accelerating the merging of the epitaxial layers and improving the surface smoothness of the epitaxial layers.
[0070] Preferably, in step (D2), the thickness of the second roughened layer is 5-10 nm, for example, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm.
[0071] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0072] (1) Growing a composite layer on a substrate, the specific steps include:
[0073] (a) introducing a first precursor at a flow rate f1 of 5-100 sccm for 5-10 s at 500-1000° C. and 150-650 torr to form a first sub-buffer layer on the first growth layer;
[0074] (b) at 500-1000° C. and 100-600 torr, a second precursor with a flow rate f2 of 5-100 sccm and a third precursor with a flow rate f3 of 20-100 slm are introduced simultaneously within 2-5 s, and then at 500-1000° C. and 100-600 torr, a second precursor with a flow rate f4 of 5-100 sccm and a third precursor with a flow rate f5 of 20-100 slm are introduced simultaneously within 5-10 s to form a second sub-buffer layer on the first sub-buffer layer;
[0075] (c) repeating steps (a) and (b) alternately to obtain the composite layer having a thickness of 5-20 nm;
[0076] Wherein, the first growth layer is the substrate or the second sub-buffer layer in the buffer layer generated in the previous step (b), f2<f4<f1, f5<f3;
[0077] (2) growing a roughened layer on the composite layer, the specific steps comprising:
[0078] (A2) thermally annealing the third growth layer at 1080-1100° C. and 150-650 torr for 2-5 seconds;
[0079] (B2) growing a first roughening layer with a thickness of 10-20 nm on the third growth layer at 1050-1060° C. and 150-650 torr;
[0080] (C2) growing a second roughening layer with a thickness of 5-10 nm on the first roughening layer at 1060-1080° C. and 150-650 torr;
[0081] (D2) repeating steps (A2) to (C2) alternately to obtain a roughened layer of step (2) having a thickness of 20-2500 nm;
[0082] The third growth layer is the composite layer or the second roughened layer generated in the previous step (C2).
[0083] (3) Growing an epitaxial layer on the roughened layer at 1100-1200° C. and 100-400 torr.
[0084] In a second aspect, the present invention provides an epitaxial wafer prepared by the preparation method as described in the first aspect, wherein the epitaxial wafer comprises a substrate, a composite layer, a roughened layer and an epitaxial layer stacked in sequence, the composite layer comprises a plurality of stacked buffer layers, and the buffer layer comprises a first sub-buffer layer and a second sub-buffer layer stacked in sequence.
[0085] Preferably, the thickness of the composite layer is 5-20 nm, for example, it may be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm or 20 nm.
[0086] Preferably, the thickness of the roughening layer is 20-2500nm, for example, it can be 20nm, 30nm, 40nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, 500nm, 1000nm, 1500nm, 2000nm or 2500nm, etc., preferably 50-100nm.
[0087] Preferably, the thickness of the epitaxial layer is 100-500 nm, for example, it may be 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 135 nm, 140 nm, 145 nm or 150 nm.
[0088] It should be noted that the technical solution provided by the present invention is also applicable to epitaxial layers with a thickness greater than 500nm, and compared with conventional growth processes, the present invention can obtain higher crystal quality. However, compared with conventional processes, the effect of the thickness of the epitaxial layer of the present invention on the crystal quality is different from that of conventional nitride epitaxial layers, because the present invention can form a composite layer with good stability, consistent phase and uniform distribution, which improves the nucleation uniformity of the composite layer, and on the basis of the composite layer, optimizes the growth process of the roughened layer, adjusts the longitudinal and lateral growth modes of the roughened layer, reduces dislocations in the epitaxial layer, and improves the crystal quality of the epitaxial layer. Therefore, although when the thickness of the epitaxial layer of the present invention is greater than 2.5μm, as the thickness continues to increase, the reduction in crystal quality is not as obvious as in conventional processes, but the dislocation density in the epitaxial layer of the present invention will be more than 30% lower at the same thickness.
[0089] Preferably, the surface roughness of the epitaxial layer is 0-100 nm, for example, it can be 0, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0090] Preferably, the composite layer, the roughened layer and the epitaxial layer are independently made of III AVA group materials.
[0091] Preferably, the III AVA group material includes any one of GaN, AlN, AlGaN, AlInN, AlGaInN, InN or InGaN, or a combination of at least two thereof.
[0092] In a third aspect, the present invention provides an electronic device, comprising the epitaxial wafer as described in the second aspect.
[0093] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0094] Compared with the prior art, the present invention has the following beneficial effects:
[0095] The present invention optimizes the preparation process of the buffer layer by controlling the inlet flow rate f1 of the first precursor to be greater than the inlet flow rate f2 of the second precursor, thereby finally forming a composite layer with good stability, consistent phase and uniform distribution, improving the nucleation uniformity of the buffer layer, providing a growth template for the subsequent growth of a roughened layer and an epitaxial layer, and finally obtaining a high-quality epitaxial layer with a smooth surface, thereby overcoming the problem of large surface roughness of a thin epitaxial layer grown in a conventional epitaxial growth process; moreover, the present invention does not need to adopt a conventional process to grow a thicker epitaxial layer to improve the crystal quality of the epitaxial layer, thereby achieving the growth of a high-quality ultra-thin epitaxial layer, effectively reducing the cost of epitaxial production, and improving the cost competitiveness of epitaxial products. BRIEF DESCRIPTION OF THE DRAWINGS
[0096] Figure 1 The present invention provides a schematic flow chart of the epitaxial wafer preparation method.
[0097] Figure 2 This is a schematic diagram of the structure of the epitaxial wafer provided in Example 1 of the present invention.
[0098] Figure 3 Schematic diagram of the structure of the composite layer in Example 1 of the present invention.
[0099] Figure 4 This is the surface AFM image of the epitaxial layer prepared in Example 1.
[0100] Figure 5 This is the surface AFM image of the epitaxial layer prepared in Example 2.
[0101] Figure 6 This is the surface AFM image of the epitaxial layer prepared in Example 3.
[0102] Figure 7 This is the surface AFM image of the epitaxial layer prepared in Example 4.
[0103] Figure 8 This is the surface AFM image of the epitaxial layer prepared in Example 5.
[0104] Fig. 9 This is the surface AFM image of the epitaxial layer prepared in Comparative Example 1.
[0105] Fig.10 This is the surface AFM image of the epitaxial layer prepared in Comparative Example 2.
[0106] Fig.11 This is the surface AFM image of the epitaxial layer prepared in Comparative Example 3.
[0107] Among them, 1 is substrate; 2 is composite layer; 21 is first buffer layer; 22 is second buffer layer; 21a is first sub-buffer layer; 21b is second buffer layer; 3 is roughened layer; 4 is epitaxial layer. DETAILED DESCRIPTION
[0108] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0109] Figure 1 The schematic diagram of the process of the epitaxial wafer preparation method provided by the present invention is shown. As can be seen from the figure, the epitaxial wafer preparation method includes the following steps:
[0110] S1: growing a composite layer on a substrate, wherein the composite layer comprises a plurality of stacked buffer layers, the buffer layer comprises a first sub-buffer layer and a second sub-buffer layer which are stacked, the first sub-buffer layer is formed by introducing a first precursor, the second sub-buffer layer is formed by introducing a second precursor and a third precursor, and an incoming flow rate f1 of the first precursor is greater than an incoming flow rate f2 of the second precursor.
[0111] The substrate may be a sapphire substrate.
[0112] S2: Growing a roughened layer on the composite layer.
[0113] S3: growing an epitaxial layer on the roughened layer.
[0114] The present invention optimizes the preparation process of the buffer layer by controlling the inlet flow rate f1 of the first precursor to be greater than the inlet flow rate f2 of the second precursor, thereby finally forming a composite layer with good stability, consistent phase and uniform distribution, improving the nucleation uniformity of the buffer layer, providing a growth template for the subsequent growth of a roughened layer and an epitaxial layer, and finally obtaining a high-quality epitaxial layer with a smooth surface, thereby overcoming the problem of large surface roughness of a thin epitaxial layer grown in a conventional epitaxial growth process; moreover, the present invention does not need to adopt a conventional process to grow a thicker epitaxial layer to improve the crystal quality of the epitaxial layer, thereby achieving the growth of a high-quality ultra-thin epitaxial layer, effectively reducing the cost of epitaxial production, and improving the cost competitiveness of epitaxial products.
[0115] Example 1
[0116] This embodiment provides an epitaxial wafer, the structural schematic diagram of the epitaxial wafer is as follows Figure 2 As shown, the epitaxial wafer includes a substrate 1, a composite layer 2, a roughened layer 3 and an epitaxial layer 4 which are grown in sequence; the structural schematic diagram of the composite layer 2 is shown in Figure 3 As shown, the composite layer 2 includes a first buffer layer 21 and a second buffer layer 22 grown in sequence, the first buffer layer 21 includes a first sub-buffer layer 21a and a second sub-buffer layer 21b grown in sequence, and the second buffer layer 22 includes a first sub-buffer layer 21a and a second sub-buffer layer 21b grown in sequence.
[0117] This embodiment also provides a method for preparing an epitaxial wafer, the method comprising the following steps:
[0118] (1) A substrate 1 is provided, and a composite layer 2 is grown on the substrate 1.
[0119] The substrate 1 is a sapphire substrate 1 with a size of 4 inches. The following steps can be used to grow the composite layer 2 on the sapphire substrate 1:
[0120] (a) Under the conditions of a temperature of 750° C. and a pressure of 200 torr, a first precursor with a flow rate f1 of 75 sccm is introduced for 8 s to form a first sub-buffer layer 21 a on the substrate 1 .
[0121] The first precursor is trimethyl gallium (TMG).
[0122] (b) at a temperature of 560° C. and a pressure of 500 torr, a second precursor with a flow rate f2 of 45 sccm and a third precursor with a flow rate f3 of 55 slm are introduced simultaneously within 3 s; then at a temperature of 560° C. and a pressure of 500 torr, a second precursor with a flow rate f4 of 50 sccm and a third precursor with a flow rate f5 of 45 slm are introduced simultaneously within 8 s to form a second sub-buffer layer 21 b on the first sub-buffer layer 21 a. The combination of the first sub-buffer layer 21 a and the second sub-buffer layer 21 b is recorded as the first buffer layer 21;
[0123] The second precursor is TMG, and the third precursor is NH3.
[0124] (c) Under the conditions of a temperature of 750° C. and a pressure of 200 torr, a first precursor with a flow rate f1 of 75 sccm is introduced for 8 s to form a first sub-buffer layer 21 a on the surface of the first buffer layer 21 .
[0125] (d) Under the conditions of temperature of 560°C and pressure of 500 torr, a second precursor TMG with a flow rate f2 of 45 sccm and a third precursor NH3 with a flow rate f3 of 55 slm are introduced simultaneously within 3 s; then, under the conditions of temperature of 560°C and pressure of 500 torr, a second precursor TMG with a flow rate f4 of 50 sccm and a third precursor NH3 with a flow rate f5 of 45 slm are introduced simultaneously within 8 s to form a second sub-buffer layer 21b on the first sub-buffer layer 21a. The combination of the first sub-buffer layer 21a and the second sub-buffer layer 21b is denoted as the second buffer layer 22, and the combination of the first buffer layer 21 and the second buffer layer 22 is denoted as the composite layer 2, i.e., the GaN composite layer, with a thickness of 15 nm.
[0126] (2) Growing a roughened layer 3 on the GaN composite layer 2, the specific steps include:
[0127] (A2) The third growth layer is subjected to a thermal annealing treatment at a temperature of 1090° C. and a pressure of 200 torr for 3 seconds.
[0128] (B2) A first roughened layer with a thickness of 15 nm was grown on the third growth layer at a temperature of 1055° C. and a pressure of 600 torr.
[0129] (C2) A second rough layer with a thickness of 7.5 nm was grown on the first rough layer at a temperature of 1075° C. and a pressure of 200 torr.
[0130] (D2) Repeat steps (A2)-(C2) alternately until a roughening layer 3 with a thickness of 80 nm, namely a GaN roughening layer, is grown.
[0131] The third growth layer is a GaN composite layer or the second roughened layer generated in the previous step (C2).
[0132] (3) Growing epitaxial layer 4 on GaN roughened layer 3 at a temperature of 1115° C. and a pressure of 150 torr.
[0133] The material of the epitaxial layer 4 is GaN, which is referred to as a GaN epitaxial layer. The thickness of the GaN epitaxial layer is 450 nm.
[0134] Example 2
[0135] The difference between this embodiment and embodiment 1 is that the growth thickness of the epitaxial layer in step (3) is 2500 nm.
[0136] The rest of the preparation methods and parameters were the same as those in Example 1.
[0137] Example 3
[0138] The difference between this embodiment and embodiment 1 is that the growth thickness of the epitaxial layer in step (3) is 500 nm.
[0139] The rest of the preparation methods and parameters were the same as those in Example 1.
[0140] Example 4
[0141] The difference between this embodiment and embodiment 1 is that the growth thickness of the epitaxial layer in step (3) is 300 nm.
[0142] The rest of the preparation methods and parameters were the same as those in Example 1.
[0143] Example 5
[0144] The difference between this embodiment and embodiment 1 is that the growth thickness of the epitaxial layer in step (3) is 100 nm.
[0145] The rest of the preparation methods and parameters were the same as those in Example 1.
[0146] Figure 4 , Figure 5 , Figure 6 , Figure 7 and Figure 8 The surface AFM image of the epitaxial layer prepared in Example 1-5 is shown. It can be seen from the image that the surface of the epitaxial layer prepared in Example 1-5 is smooth and has low roughness.
[0147] Example 6
[0148] The present embodiment provides an epitaxial wafer, which includes a substrate, a composite layer, a roughened layer and an epitaxial layer that are grown in sequence; the composite layer includes a first buffer layer and a second buffer layer that are grown in sequence, the first buffer layer includes a first sub-buffer layer and a second sub-buffer layer that are grown in sequence, and the second buffer layer includes a first sub-buffer layer and a second sub-buffer layer that are grown in sequence.
[0149] This embodiment also provides a method for preparing an epitaxial wafer, the method comprising the following steps:
[0150] (1) A substrate is provided and a composite layer is grown on the substrate.
[0151] The substrate is a sapphire substrate with a size of 4 inches. The composite layer is grown on the sapphire substrate. The specific steps include:
[0152] (a) Under the conditions of a temperature of 500° C. and a pressure of 400 torr, a first precursor with a flow rate f1 of 10 sccm is introduced for 10 s to form a first sub-buffer layer on the substrate.
[0153] The first precursor is trimethylindium.
[0154] (b) Under the conditions of a temperature of 750°C and a pressure of 350 torr, a second precursor with a flow rate f2 of 5 sccm and a third precursor with a flow rate f3 of 30 slm are simultaneously introduced within 5 s; then, under the conditions of 750°C and 350 torr, a second precursor with a flow rate f4 of 7 sccm and a third precursor with a flow rate f5 of 20 slm are simultaneously introduced within 10 s to form a second sub-buffer layer on the first sub-buffer layer.
[0155] The combination of the first sub-buffer layer and the second sub-buffer layer is recorded as the first buffer layer; the second precursor is trimethylindium, and the third precursor is n-propylamine.
[0156] (c) Under the conditions of a temperature of 500° C. and a pressure of 400 torr, a first precursor with a flow rate f1 of 10 sccm is introduced for 10 s to form a first sub-buffer layer on the surface of the first buffer layer.
[0157] (d) Under the conditions of a temperature of 750°C and a pressure of 350 torr, a second precursor with a flow rate f2 of 5 sccm and a third precursor with a flow rate f3 of 30 slm are simultaneously introduced within 5 s; then, under the conditions of 750°C and 350 torr, a second precursor with a flow rate f4 of 7 sccm and a third precursor with a flow rate f5 of 20 slm are simultaneously introduced within 10 s to form a second sub-buffer layer on the first sub-buffer layer.
[0158] The combination of the first sub-buffer layer and the second sub-buffer layer is recorded as the second buffer layer, and the combination of the first buffer layer and the second buffer layer is recorded as a composite layer, that is, an InN composite layer, with a thickness of 5 nm.
[0159] (2) Growing a roughened layer on the composite layer, the specific steps include:
[0160] (A2) The third growth layer is thermally annealed at a temperature of 1080° C. and a pressure of 400 torr for 5 seconds.
[0161] (B2) A first roughened layer with a thickness of 10 nm was grown on the third growth layer at a temperature of 1050° C. and a pressure of 400 torr.
[0162] (C2) A second rough layer with a thickness of 7 nm was grown on the first rough layer at a temperature of 1060° C. and a pressure of 400 torr.
[0163] (D2) Repeating steps (A2)-(C2) alternately to obtain a roughened layer of step (2) with a thickness of 50 nm;
[0164] The third growth layer is an InN composite layer or the second roughened layer generated in the previous step (C2).
[0165] (3) growing an epitaxial layer on the roughened layer at a temperature of 1115°C and a pressure of 250 torr;
[0166] The material of the epitaxial layer is InN, which is referred to as an InN epitaxial layer. The thickness of the InN epitaxial layer is 150 nm.
[0167] Example 7
[0168] The present embodiment provides an epitaxial wafer, which includes a substrate, a composite layer, a roughened layer and an epitaxial layer that are grown in sequence; the composite layer includes a first buffer layer and a second buffer layer that are grown in sequence, the first buffer layer includes a first sub-buffer layer and a second sub-buffer layer that are grown in sequence, and the second buffer layer includes a first sub-buffer layer and a second sub-buffer layer that are grown in sequence.
[0169] This embodiment also provides a method for preparing an epitaxial wafer, the method comprising the following steps:
[0170] (1) A substrate is provided and a composite layer is grown on the substrate.
[0171] The substrate is a sapphire substrate, the size of which may be 4 inches. The composite layer is grown on the sapphire substrate. The specific steps include:
[0172] (a) A first precursor with a flow rate f1 of 100 sccm is introduced at a temperature of 1000° C. and a pressure of 650 torr for 5 seconds to form a first sub-buffer layer on the substrate.
[0173] The first precursor is trimethylaluminum.
[0174] (b) Under the conditions of a temperature of 1000°C and a pressure of 100 torr, a second precursor with a flow rate f2 of 90 sccm and a third precursor with a flow rate f3 of 100 slm are simultaneously introduced within 2 s; then, under the conditions of 1000°C and 100 torr, a second precursor with a flow rate f4 of 95 sccm and a third precursor with a flow rate f5 of 90 slm are simultaneously introduced within 5 s to form a second sub-buffer layer on the first sub-buffer layer. The combination of the first sub-buffer layer and the second sub-buffer layer is recorded as the first buffer layer.
[0175] The second precursor is trimethylaluminum, and the third precursor is dimethylhydrazine.
[0176] (c) introducing a first precursor at a flow rate f1 of 100 sccm for 5 s at a temperature of 1000° C. and a pressure of 650 torr to form a first sub-buffer layer on the surface of the first buffer layer.
[0177] (d) Under the conditions of a temperature of 1000°C and a pressure of 100 torr, a second precursor with a flow rate f2 of 90 sccm and a third precursor with a flow rate f3 of 100 slm are simultaneously introduced within 2 s; then, under the conditions of 1000°C and 100 torr, a second precursor with a flow rate f4 of 95 sccm and a third precursor with a flow rate f5 of 90 slm are simultaneously introduced within 5 s to form a second sub-buffer layer on the first sub-buffer layer.
[0178] The combination of the first sub-buffer layer and the second sub-buffer layer is recorded as the second buffer layer, and the combination of the first buffer layer and the second buffer layer is recorded as a composite layer, that is, an AlN composite layer, with a thickness of 20 nm.
[0179] (2) Growing a roughened layer on the composite layer, the specific steps include:
[0180] (A2) The third growth layer is thermally annealed at a temperature of 1100° C. and a pressure of 650 torr for 2 seconds.
[0181] (B2) A first roughened layer with a thickness of 20 nm was grown on the third growth layer at a temperature of 1060° C. and a pressure of 200 torr.
[0182] (C2) A second rough layer with a thickness of 10 nm is grown on the first rough layer at a temperature of 1080° C. and a pressure of 600 torr.
[0183] (D2) Repeat steps (A2) to (C2) alternately to obtain a roughened layer of step (2) with a thickness of 100 nm, i.e., an AlN roughened layer.
[0184] The third growth layer is an AlN composite layer or the second roughened layer generated in the previous step (C2).
[0185] (3) Growing an epitaxial layer on the roughened layer at 1115°C and 400 torr.
[0186] The material of the epitaxial layer is AlN, which is referred to as AlN epitaxial layer. The thickness of the AlN epitaxial layer is 250 nm.
[0187] Example 8
[0188] The difference between this embodiment and embodiment 1 is that f4 in step (b) is 80 sccm.
[0189] The rest of the preparation methods and parameters were the same as those in Example 1.
[0190] Example 9
[0191] The difference between this embodiment and embodiment 1 is that in step (b), f4 is 40 sccm.
[0192] The rest of the preparation methods and parameters were the same as those in Example 1.
[0193] Example 10
[0194] The difference between this embodiment and embodiment 1 is that f5 in step (b) is 60 sccm.
[0195] The rest of the preparation methods and parameters were the same as those in Example 1.
[0196] Embodiment 11
[0197] The difference between this embodiment and Embodiment 1 is that the "steps (A2)-(C2)" repeated and alternating in step (D2) are modified to "steps (B2)-(C2)", that is, the repeated steps do not include thermal annealing, and only the repeated alternating growth of the first roughened layer and the second roughened layer is performed.
[0198] The rest of the preparation methods and parameters were the same as those in Example 1.
[0199] Comparative Example 1
[0200] This comparative example adopts a conventional 4-inch mass production process to grow a GaN epitaxial layer with a thickness of 4.5 μm. The specific steps are as follows:
[0201] (1) Provide 4-inch sapphire substrate.
[0202] (2) Under the conditions of temperature of 560°C and pressure of 500 torr, TMG and NH3 were introduced to grow a GaN buffer layer with a thickness of 15 nm.
[0203] (3) A GaN roughening layer with a thickness of 1 μm is grown on the GaN buffer layer at a temperature of 1055°C and a pressure of 600 torr.
[0204] (4) A GaN epitaxial layer with a thickness of 4.5 μm is grown on the GaN roughened layer at a temperature of 1115° C. and a pressure of 150 torr.
[0205] Comparative Example 2
[0206] The difference between this comparative example and comparative example 1 is that the growth thickness of the GaN epitaxial layer is 2.5 μm.
[0207] The rest of the preparation methods and parameters were the same as those in Comparative Example 1.
[0208] Comparative Example 3
[0209] The difference between this comparative example and comparative example 1 is that the growth thickness of the GaN epitaxial layer is 0.5 μm.
[0210] The rest of the preparation methods and parameters were the same as those in Comparative Example 1.
[0211] Fig. 9 , Fig.10 and Fig.11 The surface AFM images of the epitaxial layers prepared in Comparative Examples 1-3 are shown. It can be seen from the images that as the thickness of the epitaxial layer decreases, the number of pit-shaped defects on the surface of the epitaxial layer increases. When the thickness of the epitaxial layer is 0.5 μm, the surface has a large number of defects.
[0212] Comparative Example 4
[0213] The difference between this comparative example and Example 1 is that f2 is 80 sccm, that is, the inlet flow rate f1 of the first precursor is smaller than the inlet flow rate f2 of the second precursor.
[0214] The rest of the preparation methods and parameters were the same as those in Example 1.
[0215] Comparative Example 5
[0216] The difference between this comparative example and Example 1 is that f2 is 75 sccm, that is, the inlet flow rate f1 of the first precursor is equal to the inlet flow rate f2 of the second precursor.
[0217] The rest of the preparation methods and parameters were the same as those in Example 1.
[0218] Performance Testing
[0219] The epitaxial wafers prepared in Examples 1-11 and Comparative Examples 1-5 were subjected to an atomic force microscope (AFM) surface roughness Ra test and an X-ray diffraction (XRD) test.
[0220] The test results are shown in Table 1:
[0221] Table 1
[0222]
[0223]
[0224] It can be seen from the above table that, on the one hand, the present invention forms a composite layer with good stability, consistent phase and uniform distribution by optimizing the preparation process of the buffer layer, thereby improving the nucleation uniformity of the buffer layer and providing a growth template for the subsequent growth of the roughened layer and the epitaxial layer; on the other hand, on the basis of the composite layer, through the process optimization of the roughened layer, the longitudinal and lateral growth modes of the roughened layer are adjusted, and a growth template is provided for the subsequent growth of the epitaxial layer, and finally a high-quality epitaxial layer with a smooth surface is obtained, which overcomes the problem of large surface roughness of the thin epitaxial layer grown in the conventional epitaxial growth process; moreover, the present invention does not need to adopt conventional processes to grow a thicker epitaxial layer to improve the crystal quality of the epitaxial layer, and realizes the growth of high-quality ultra-thin epitaxial layers, effectively reducing the cost of epitaxial production and improving the cost competitiveness of epitaxial products.
[0225] By comparing the data results of Example 1 with those of Examples 8-9, it can be seen that if f4 is greater than f1, the growth of the composite layer will be uneven, thereby increasing the roughness of the epitaxial layer and reducing the crystal quality of the epitaxial layer; if f4 is less than f2, the Ga surface distribution of the composite layer will gradually shift to the N surface, reducing the surface stability, thereby increasing the roughness of the epitaxial layer and reducing the crystal quality of the epitaxial layer.
[0226] From the comparison of the data results of Example 1 and Example 10, it can be seen that if f5 is greater than f3, the Ga surface distribution of the composite layer will gradually shift to the N surface, reducing the surface stability, thereby increasing the roughness of the epitaxial layer and reducing the crystal quality of the epitaxial layer.
[0227] By comparing the data results of Example 1 with those of Example 11, it can be seen that if only steps (B2)-(C2) are repeated during the growth of the composite layer, the longitudinal coarsening effect of the second coarsening layer will be weakened, the merging process of the epitaxial layer will be accelerated, the probability of dislocation turning will be reduced, and the crystal quality of the epitaxial layer will be reduced to a certain extent.
[0228] By comparing the data results of Example 1 with those of Comparative Example 1, it can be seen that if conventional processes are used to grow the epitaxial layer, the nucleation uniformity is poor and the degree of surface merging varies greatly during the growth of the epitaxial layer, which increases the roughness of the epitaxial layer and reduces the crystal quality of the epitaxial layer.
[0229] By comparing the data results of Comparative Example 1 with Comparative Examples 2-3, it can be seen that if the conventional process is used to grow the epitaxial layer, as the thickness of the epitaxial layer decreases, the half-peak width of the (102) plane diffraction gradually increases, indicating that the crystal quality of the epitaxial layer will become worse and worse as the thickness decreases.
[0230] By comparing the data results of Comparative Example 1 with Comparative Examples 4-5, it can be seen that if the flow rate f1 of the first precursor is less than or equal to the flow rate f2 of the second precursor, the coverage uniformity of the III A group precursor will deteriorate, resulting in poor uniformity of the composite layer, which will also increase the roughness of the epitaxial layer and reduce the crystal quality of the epitaxial layer.
[0231] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an epitaxial wafer, characterized in that: The preparation method comprises the following steps: (1) growing a composite layer on a substrate, wherein the composite layer comprises a plurality of stacked buffer layers, the buffer layer comprises a first sub-buffer layer and a second sub-buffer layer which are stacked, the first sub-buffer layer is formed by introducing a first precursor, the second sub-buffer layer is formed by introducing a second precursor and a third precursor, and an introduction flow rate f1 of the first precursor is greater than an introduction flow rate f2 of the second precursor; (2) growing a roughened layer on the composite layer; (3) Growing an epitaxial layer on the roughened layer.
2. The preparation method according to claim 1, characterized in that: The step (1) specifically comprises: (a) introducing a first precursor to form a first sub-buffer layer on the first growth layer; (b) introducing a second precursor and a third precursor to form a second sub-buffer layer on the first sub-buffer layer; (c) repeating steps (a) and (b) alternately to obtain the composite layer; The first growth layer is the substrate or the second sub-buffer layer formed in the previous step (b).
3. The preparation method according to claim 1 or 2, characterized in that: Step (1) The first precursor and the second precursor are independently group IIIA organic source precursors; Preferably, the third precursor in step (1) is a group VA source precursor.
4. The preparation method according to claim 2 or 3, characterized in that: Step (a) The flow rate f1 of the first precursor is 5-100 sccm; Preferably, the time for introducing the first precursor in step (a) is 5-10 seconds; Preferably, the step (b) specifically comprises: (b1) introducing a second precursor with a flow rate of f2 and a third precursor with a flow rate of f3 under the first set condition; (b2) introducing a second precursor with a flow rate of f4 and a third precursor with a flow rate of f5 under a second set condition; Preferably, in the first setting condition, the temperature is 500-1000°C and the time is 2-5s; Preferably, in the second setting condition, the temperature is 500-1000°C and the time is 5-10s; Preferably, in step (b), f2<f4<f1; Preferably, in step (b), f2 is 5-100 sccm; Preferably, in step (b), f4 is 5-100 sccm; Preferably, in step (b), f5<f3; Preferably, in step (b), f3 is 20-100 slm; Preferably, in step (b), f5 is 20-100 slm.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The step (2) specifically comprises: (A1) thermally annealing the composite layer; (B1) growing a first roughened layer on the second grown layer under a third setting condition; (C1) growing a second rough layer on the first rough layer under fourth setting conditions; (D1) Repeating steps (B1) to (C1) alternately to obtain the roughened layer described in step (2); The second growth layer is the composite layer or the second roughened layer generated in the previous step (C1).
6. The preparation method according to any one of claims 1 to 4, characterized in that: The step (2) specifically comprises: (A2) thermally annealing the third growth layer; (B2) growing a first roughened layer on the third grown layer under a third set condition; (C2) growing a second rough layer on the first rough layer under fourth setting conditions; (D2) Repeating steps (A2) to (C2) alternately to obtain the roughened layer described in step (2); The third growth layer is the composite layer or the second roughened layer generated in the previous step (C2).
7. The preparation method according to claim 6, characterized in that: The temperature of the thermal annealing in step (A2) is 1080-1100° C.; Preferably, the thermal annealing time in step (A2) is 2-5s; Preferably, in the third setting condition of step (B2), the temperature is 1050-1060°C; Preferably, in step (B2), the thickness of the first roughened layer is 10-20 nm; Preferably, in the fourth setting condition of step (C2), the temperature is 1060-1080°C; Preferably, in step (D2), the thickness of the second roughened layer is 5-10 nm.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) Growing a composite layer on a substrate, the specific steps include: (a) introducing a first precursor at a flow rate f1 of 5-100 sccm for 5-10 s at 500-1000° C. and 150-650 torr to form a first sub-buffer layer on the first growth layer; (b) at 500-1000° C. and 100-600 torr, a second precursor with a flow rate f2 of 5-100 sccm and a third precursor with a flow rate f3 of 20-100 slm are introduced simultaneously within 2-5 s, and then at 500-1000° C. and 100-600 torr, a second precursor with a flow rate f4 of 5-100 sccm and a third precursor with a flow rate f5 of 20-100 slm are introduced simultaneously within 5-10 s to form a second sub-buffer layer on the first sub-buffer layer; (c) repeating steps (a) and (b) alternately to obtain the composite layer having a thickness of 5-20 nm; Wherein, the first growth layer is the substrate or the second sub-buffer layer in the buffer layer generated in the previous step (b), f2<f4<f1, f5<f3; (2) growing a roughened layer on the composite layer, the specific steps comprising: (A2) thermally annealing the third growth layer at 1080-1100° C. and 150-650 torr for 2-5 seconds; (B2) growing a first roughening layer with a thickness of 10-20 nm on the third growth layer at 1050-1060° C. and 150-650 torr; (C2) growing a second roughening layer with a thickness of 5-10 nm on the first roughening layer at 1060-1080° C. and 150-650 torr; (D2) repeating steps (A2) to (C2) alternately to obtain a roughened layer of step (2) having a thickness of 50-2500 nm; Wherein, the third growth layer is the composite layer or the second roughened layer generated in the previous step (C2); (3) Growing an epitaxial layer on the roughened layer at 1100-1200° C. and 100-400 torr.
9. An epitaxial wafer prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The epitaxial wafer comprises a substrate, a composite layer, a roughened layer and an epitaxial layer which are stacked in sequence, the composite layer comprises a plurality of stacked buffer layers, and the buffer layer comprises a first sub-buffer layer and a second sub-buffer layer which are stacked; Preferably, the thickness of the composite layer is 5-20 nm; Preferably, the thickness of the roughening layer is 20-2500 nm, preferably 50-100 nm; Preferably, the thickness of the epitaxial layer is 100-500 nm; Preferably, the surface roughness of the epitaxial layer is 0-100 nm; Preferably, the composite layer, the roughened layer and the epitaxial layer are independently IIIA-V A group materials.
10. An electronic device, characterized in that: The electronic device comprises the epitaxial wafer as claimed in claim 9.