Single-crystal positive electrode material and preparation method thereof
The single crystal positive electrode material synthesized by three-step calcination method solves the problems of low discharge capacity and high residual alkali of high nickel positive electrode material, achieves efficient and low-cost battery performance improvement, avoids bloating, and provides excellent capacity and cycle performance.
Patent Information
- Application Number
- CN202411176570.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing high-nickel ternary single-crystal cathode materials have problems with low discharge capacity, high residual alkali, and flatulence. The traditional synthesis method leads to uneven primary particles, poor structural morphology, and high cost, which cannot meet the performance requirements of high-efficiency batteries.
By adjusting the molar ratio and calcining conditions of the lithium source and the precursor, controlling the oxygen concentration and the pressure difference in the furnace, synthesizing a single crystal positive electrode material with a loose porous structure, reducing the residual alkali and increasing the primary particles. Uniformity and battery performance.
The high capacity, excellent circulation performance and low-cost production of single crystal positive electrode materials are achieved, which avoids the problem of high temperature inflation and improves the stability and circulation performance of the battery.
Smart Images

Figure CN119061478A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of batteries, and in particular relates to a single crystal positive electrode material and a preparation method thereof. Background Art
[0002] As a new type of energy storage and conversion device, lithium-ion batteries have the advantages of high operating voltage, high energy / power density, long cycle life and environmental friendliness. They are widely used in portable electronic devices, energy storage grids and electric vehicles. In order to improve energy density, there are currently two main technical means used in the research and development of positive electrode ternary materials: one is to increase the nickel content of the positive electrode material, and the other is to increase the compaction density of the material. In order to increase the compaction density of the material, large particles are usually matched with small particles. Large particles use secondary particles composed of primary particles, and small particles use single crystal or quasi-single crystal positive electrode materials.
[0003] The capacity of high-nickel cathode materials increases with the increase of nickel content. However, due to the high nickel content, high-valent nickel ions are highly oxidizing and alkaline, which increases the side reactions on the particle surface, reduces its structural stability, and causes serious gas production. + 、Ni 2 + Mixing reduces Li + The diffusion coefficient makes the rate performance of the material worse. Due to the mixing, the Li + The specific capacity also decreases as the nickel ion content increases. As the phase change becomes more serious, microcracks appear on the particle surface, accompanied by the formation of NiO rock salt phase, which reduces the material's cycle performance. This phenomenon is more serious compared to the secondary particles composed of single crystal high nickel positive electrode materials and primary particles.
[0004] High nickel ternary single crystals have the following unavoidable defects: 1. Low discharge capacity; 2. High residual alkali; 3. Poor single crystal morphology leading to flatulence problems.
[0005] The traditional synthesis method of high-nickel ternary single crystal positive electrode materials has defects: 1. The lithium salt and additives are mixed with the precursor at one time, and then calcined at high temperature, which easily leads to uneven primary particle size, poor single crystal structure morphology, high residual alkali, low capacity and other phenomena; 2. Conventional high-nickel single crystals are calcined in a pure oxygen atmosphere, which causes a huge waste of cost, and in a pure oxygen environment, the primary particles are small and difficult to form crystals. At the same time, the traditional synthesis method cannot meet the needs of synthesizing single crystal materials, and the subsequent coating improvement is not a good method. Summary of the invention
[0006] Therefore, the technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art, thereby providing a single crystal positive electrode material and a preparation method thereof.
[0007] The first aspect of the present invention provides a method for preparing a single crystal positive electrode material, wherein the preparation steps include:
[0008] S1, mixing a precursor, a first lithium source, and a first additive, wherein the ratio of the total molar number of lithium element in the first lithium source to the total molar number of metal element in the precursor is a:1, 0.9<a<1.0, and performing a first calcination to obtain a calcined product;
[0009] Among them, the temperature rising section, constant temperature section and temperature falling section of the first calcination are ventilated with air; the pressure difference in the furnace is -20 to -3Pa;
[0010] S2, mixing the first calcined product, the second lithium source, and the second additive, wherein the ratio of the total molar number of the lithium element in the second lithium source to the total molar number of the metal element in the first calcined product is a':1, 0<a'≤0.06, and performing a second calcination to obtain a second calcined product;
[0011] The second calcination has no ventilation in the heating section, air in the constant temperature section, and oxygen in the cooling section; the pressure difference in the furnace in the heating section is -12 to -3Pa, the pressure difference in the furnace in the constant temperature section is -5 to 3Pa, and the pressure difference in the furnace in the cooling section is 0-10Pa;
[0012] S3, mixing the second calcined product, the third lithium source, and the third additive, wherein the ratio of the total molar number of the lithium element in the third lithium source to the total molar number of the metal element in the second calcined product is 0<a″≤0.05, and performing a third calcination to obtain a single crystal positive electrode material;
[0013] Among them, the temperature rising section and constant temperature section of the third calcination are not ventilated, and oxygen is ventilated in the temperature falling section; the pressure difference in the furnace in the temperature falling section is 1-5Pa.
[0014] In the present invention, the first lithium source, the second lithium source and the third lithium source are conventional lithium sources in the art. Typically, but not limiting, the first lithium source, the second lithium source and the third lithium source each independently include LiOH and Li2CO3.
[0015] In the present invention, the first calcination, the second calcination and the third calcination each independently include a heating section, a constant temperature section and a cooling section; when the heating section and the constant temperature section are not ventilated, the pressure difference in different sintering stages is controlled by adjusting the air intake flow rate and the fan frequency at the head and tail of the furnace, thereby controlling the flow direction of the gas. The gas (oxygen and / or air) in the cooling section will flow into the constant temperature section and the heating section to form an oxygen and / or air atmosphere, which is different from directly introducing oxygen and / or air. It can not only form an oxygen concentration curve, which is beneficial to the synthesis of single crystal positive electrode materials, but also reduce costs; the pressure difference in the furnace is not a fixed value, and generally fluctuates by 1-2°C during specific experiments.
[0016] In the present invention, the mixing is a conventional mixing method in the art, and it is sufficient to mix uniformly.
[0017] According to the present invention, the average particle size of the precursor is 1-5 μm, and the specific surface area (BET) is 10-20 m 2 / g, tap density (TD) is 1.2-1.8g / cm 3 , the porosity is 30-40%.
[0018] According to the present invention, the specific conditions of the first calcination are: a heating rate of 2-6°C / min, a constant temperature of 630-730°C, and a constant temperature time of 6-12h.
[0019] According to the present invention, the total molar ratio of the metal element in the first additive to the metal element in the precursor is 0.0010-0.0050:1.
[0020] According to the present invention, the first additive includes at least one of metal oxides, metal carbonate compounds, and metal hydroxides, and can be any one of SrCO3, W2O3, ZrO2, Y2O3, Al2O3, Al(OH)3, and Co3O4.
[0021] In the present invention, when the first additive is SrCO3, W2O3, or ZrO2, the molar ratio of the Sr element in SrCO3, the W element in W2O3, and the Zr element in ZrO2 is (0.0005-0.0050):(0.0001-0.0010):(0.0005-0.0050).
[0022] According to the present invention, the specific conditions of the second calcination are: heating rate of 8-16°C / min, constant temperature of 730-830°C, constant temperature time of 6-12h; cooling rate of 2-6°C / min, and the material is taken out when the temperature drops to 100-200°C.
[0023] According to the present invention, the total molar ratio of the metal element in the second additive to the metal element in the precursor is 0.0005-0.0050:1.
[0024] According to the present invention, the second additive includes metal oxide and / or metal hydroxide, which can be any one of ZrO2, TiO2, Y2O3, Al2O3, Al(OH)3, and Co3O4.
[0025] According to the present invention, the specific conditions of the third calcination are: a heating rate of 5-10°C / min, a constant temperature of 400-700°C, and a constant temperature time of 2-6h.
[0026] According to the present invention, the total molar ratio of the metal elements in the third additive to the metal elements in the precursor is 0.0005-0.0020:1.
[0027] According to the present invention, the third additive includes at least one of boric acid, oxides, and metal hydroxides, and can be selected from any one of W2O3, ZrO2, TiO2, Y2O3, Al2O3, Al(OH)3, H3BO3, and B2O3.
[0028] In the present invention, when the third additive is W2O3 or ZrO2, the molar ratio of the W element in W2O3 to the Zr element in ZrO2 is (0.0001-0.0020):(0.0005-0.0020).
[0029] The second aspect of the present invention protects a single crystal positive electrode material, wherein the positive electrode material has a general formula of Li a+a’+a” Ni x Co y Mn z M b O2;
[0030] Among them, 0.9 <a
[0031] M is at least one of Zr, Sr, W, Ti, Y, Co, Al, and B.
[0032] In the present invention, the general formula of the precursor is Ni x Co y Mn z (OH)2, 0.8<x<1, 0<y<0.2, 0<z<0.2.
[0033] The positive electrode material of the present invention is prepared into a battery for use, and the preparation steps include:
[0034] The preparation of positive electrode sheets mainly includes pulping, coating, drying, and tableting. Slurrying refers to preparing the powdered positive electrode material into a slurry, stirring and mixing evenly on a magnetic stirrer according to the mass ratio of positive electrode material: conductive agent (acetylene black): binder (polyvinylidene fluoride, PVDF) = (94-95): (2.5-3): (2.5-3), then adding N-methylpyrrolidone (NMP), the ratio of positive electrode material to NMP is 4: 8-10g / mL, and stirring is continued for 30-40min. Use a scraper to evenly coat the slurry on one side, the scraper is 350-500μm, and after coating, it is air-dried and vacuum-dried to remove the solvent NMP and moisture. The drying temperature is 110-140℃ and the drying time is 6-10h. After coating, use a roller press to press the electrode to a thickness of 40-60 μm, cut into discs with a diameter of 13 mm, and maintain a compaction density of 2.0-2.4 g / cm 3 .
[0035] Assembly of button cell
[0036] The button half-cell is assembled in a glove box filled with argon, with a water content of less than 0.5ppm. The specific components of the electrolyte are ethylene carbonate (EC) and diethyl carbonate (DEC), and the volume ratio of EC to DEC is 1-1.05:1. The order of assembling the battery is negative electrode shell-gasket-electrolyte-lithium sheet (Ф15-17mm)-electrolyte-diaphragm (Ф18-20mm)-electrolyte-positive electrode sheet-gasket-positive electrode shell. Finally, press it for use.
[0037] Electrochemical performance test
[0038] In this project, the charging and discharging experiments of single crystal positive electrode materials were performed using Shenzhen Xinwei charging and discharging tester and CR2032 button batteries for performance testing.
[0039] The technical solution of the present invention has the following advantages:
[0040] 1. The present invention protects a method for preparing a single crystal positive electrode material, wherein the preparation steps include: S1, mixing a precursor, a first lithium source, and a first additive, wherein the ratio of the total molar number of lithium elements in the first lithium source to the total molar number of metal elements in the precursor is a:1, 0.9<a<1.0, and performing a first calcination to obtain a first calcined product; wherein the temperature rising section, the constant temperature section, and the temperature falling section of the first calcination are ventilated with air; and the pressure difference in the furnace is -20 to -3Pa; S2, mixing the first calcined product, a second lithium source, and a second additive, wherein the ratio of the total molar number of lithium elements in the second lithium source to the total molar number of metal elements in the first calcined product is a':1, 0<a'≤0.06, and performing a second calcination to obtain a second calcined product; wherein the temperature rising section of the second calcination is not ventilated, the constant temperature section is ventilated with air, and the temperature falling section is ventilated with oxygen; the pressure difference in the furnace in the temperature rising section is -12 to -3Pa, and the pressure difference in the furnace in the constant temperature section is -5 to 3Pa, the pressure difference in the furnace during the cooling period is 0-10Pa; S3, mixing the second calcined product, the third lithium source, and the third additive, wherein the ratio of the total molar number of lithium elements in the third lithium source to the total molar number of metal elements in the second calcined product is 0<a”≤0.05, and performing a third calcination to obtain a single crystal positive electrode material; wherein the heating section and the constant temperature section of the third calcination are not ventilated, and oxygen is ventilated in the cooling section; the pressure difference in the furnace during the cooling section is 1-5Pa; the preparation method of the present invention performs three step-by-step calcinations, adds a specific amount of lithium source during each calcination, and controls different oxygen concentrations and pressure differences in the furnace during the three calcinations, does not require a high-purity oxygen environment, greatly reduces production costs, reduces the amount of residual alkali on the surface of the generated positive electrode material, can accurately design the morphology of primary particles, and the battery containing the single crystal positive electrode material has good stability, will not swell in a high temperature environment, and has excellent capacity, room temperature cycle performance and high temperature cycle performance.
[0041] 2. The specific loose porous structure of the precursor in the present invention can further ensure the successful preparation of primary particles and reduce the temperature and difficulty required for the reaction.
[0042] 3. The specific first calcination conditions of the present invention can further make the metal elements in the first additive and the lithium elements in the first lithium source more evenly incorporated into the material. Instead of being enriched in the grain boundaries, they all participate in increasing the size of the primary particles. The generated primary particles are more uniform, thereby improving the performance of the battery.
[0043] 4. The specific first additive type of the present invention can further precisely control the size of the primary particles.
[0044] 5. The specific dosage of the first additive of the present invention can further increase the size of the primary particles without reducing the capacity and increasing the cost.
[0045] 6. The specific second calcination conditions of the present invention can further increase the size of the primary particles, reduce the residual alkali content, and improve the quality of the single crystal.
[0046] 7. The specific second additive type of the present invention can further reduce the residual alkali content and improve the battery cycle performance.
[0047] 8. The specific dosage of the second additive of the present invention can further improve the battery cycle performance without reducing the capacity and increasing the cost.
[0048] 9. The specific third calcination conditions of the present invention can further make the surface of the primary particles smooth, reduce the residual alkali content and make the third additive evenly coated on the surface of the positive electrode material, thereby improving the capacity and cycle performance of the positive electrode material.
[0049] 10. The specific third additive type of the present invention can further reduce the residual alkali content, evenly coat the surface of the material, and increase the capacity of the material.
[0050] 11. The specific dosage of the third additive of the present invention can reduce the residual alkali content and increase the capacity of the battery.
[0051] 12. The single crystal positive electrode material provided by the present invention, wherein the positive electrode material has the general formula of Li a+a’+a” Ni x Co y Mn z M b O2; wherein, 0.9<a<1.0, 0<a'≤0.06, 0<a”≤0.05, 1.01<a+a'+a”<1.11; 0.8<x<1.0, 0<y<0.2, 0<z<0.2 and x+y+z=1; 0<b≤0.05; M is at least one of Zr, Sr, W, Ti, Y, Co, Al, and B; the battery containing the single crystal positive electrode material has good stability and excellent capacity and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0053] Figure 1 Electron microscope image of the cross section of the precursor of Example 1;
[0054] Figure 2 Example 1: Electron microscope image of the fired product;
[0055] Figure 3 Electron microscope image of the second fired product of Example 1;
[0056] Figure 4 Electron microscope image of single crystal positive electrode material of Example 1;
[0057] Figure 5 Example 1: First cycle charge and discharge capacity;
[0058] Figure 6 Capacity retention after 50 cycles at 25°C of Example 1;
[0059] Figure 7 Electron microscope image of single crystal positive electrode material of Comparative Example 1;
[0060] Figure 8 Electron microscope image of the single crystal positive electrode material of Comparative Example 2. DETAILED DESCRIPTION
[0061] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0062] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0063] Example 1
[0064] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0065] S1, the average particle size is 2.5μm, BET is 15m 2 / g, TD is 1.5g / cm 3 , the porosity of the precursor Ni is 35% 0.95 Co 0.03 Mn 0.02 (OH)2 is mixed with LiOH, SrCO3, W2O3 and ZrO2, the molar ratio of Li element in LiOH to the total molar number of metal elements in the precursor is 0.98:1, and the molar ratio of Sr element in SrCO3, W element in W2O3, Zr element in ZrO2 and the total molar number of metal elements in the precursor is 0.0010:0.00025:0.00067:1; the mixed powder is first calcined in an atmosphere roller kiln, the temperature is increased from room temperature to 650°C at a heating rate of 5°C / min, the temperature is kept constant at 650°C for 10 hours, and then the temperature is naturally cooled to room temperature. Air is passed through the heating section, the constant temperature section and the cooling section, and the pressure difference in the furnace is maintained at -10±2Pa to obtain a sintered product.
[0066] S2. Mix all the first-burned products obtained above with LiOH and ZrO2, wherein the total molar number of Li element in LiOH to the total molar number of metal elements in the precursor is 0.05:1, and the molar ratio of Zr element in ZrO2 to the total molar number of metal elements in the precursor is 0.00067:1; the mixed powder is calcined for the second time in an atmosphere roller kiln, with no ventilation in the heating section, air in the constant temperature section, and oxygen in the cooling section. The pressure difference in the heating section is ensured to be -6±2Pa in the heating section, 0±2Pa in the constant temperature section, and 5±2Pa in the cooling section through the furnace top plug valve and the furnace head exhaust fan; the temperature is raised from room temperature to 750℃ at 9℃ / min, and the temperature is kept constant at 750℃ for 8h, and the cooling rate is controlled to be 2.5℃ / min. After the temperature is naturally cooled to 150℃, the material is taken out; after cooling to room temperature, it is crushed, sieved, and demagnetized to obtain the second-burned product.
[0067] S3. Mix all the above-prepared second-burned products with LiOH, ZrO2, and W2O3, wherein the molar ratio of the Li element in LiOH to the total molar number of metal elements in the precursor is 0.005:1, and the molar ratio of the W element in W2O3, the Zr element in ZrO2, and the total molar number of metal elements in the precursor is 0.00025:0.00067:1. Then, calcinate for the third time in an atmosphere furnace, without ventilation in the heating section and the constant temperature section, and with oxygen in the cooling section. The temperature is raised from room temperature to 550°C at a heating rate of 8°C / min, and maintained at 550°C for 4h. The pressure difference in the furnace is controlled by the furnace head exhaust fan to a pressure difference of 3±2Pa in the cooling section, to obtain Li 1.035 Ni 0.95 Co 0.0 3Mn 0.02 Zr 0.002 Sr 0.001 W 0.0005 O2 single crystal positive electrode material.
[0068] The cross-sectional morphology of the precursor is as follows Figure 1 The structure is loose and porous. Figure 2 As shown in the figure, the primary particles have been successfully prepared; the morphology of the secondary fired product is as follows Figure 3 As shown, Li 1.035 Ni 0.95 Co 0.03 Mn 0.02 Zr 0.002 Sr 0.001 W 0.0005 The morphology of O2 single crystal cathode material is as follows Figure 4 As shown, from Figure 2-4It can be seen that after the first calcination, smaller primary particles are generated and the primary particles are in an aggregated state. After the second calcination, the aggregated primary particles are separated and increased in size. After the third calcination, the surface of the primary particles becomes smoother with fewer defects.
[0069] Example 2
[0070] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0071] S1, the average particle size is 5μm, BET is 10m 2 / g, TD is 1.3g / cm 3 , the porosity of the precursor Ni is 32% 0.90 Co 0.05 Mn 0.05 (OH)2 is mixed with Li2CO3 and Al2O3, the molar ratio of Li element in Li2CO3 to the total molar number of metal elements in the precursor is 0.92:1, and the molar ratio of Al element in Al2O3 to the total molar number of metal elements in the precursor is 0.00192:1; the mixed powder is first calcined in an atmosphere roller kiln, the temperature is increased from room temperature to 700°C at a heating rate of 6°C / min, and the temperature is naturally cooled to room temperature after being kept at a constant temperature at 700°C for 6 hours. Air is passed through the heating section, the constant temperature section and the cooling section, and the pressure difference in the furnace is maintained at -15±2Pa to obtain a sintered product.
[0072] S2. Mix all the first-burned products obtained above with Li2CO3 and Y2O3, wherein the total molar ratio of the Li element in Li2CO3 to the total molar number of the metal elements in the precursor is 0.06:1, and the molar ratio of the Y element in Y2O3 to the total molar number of the metal elements in the precursor is 0.0009:1; the mixed powder is calcined for the second time in an atmosphere roller kiln, with no ventilation in the heating section, air in the constant temperature section, and oxygen in the cooling section. The pressure difference in the heating section is ensured to be -10±2Pa in the heating section, -3±2Pa in the constant temperature section, and 7±2Pa in the cooling section through the furnace top plug valve and the furnace head exhaust fan; the second calcination heating section is heated from room temperature to 800℃ at 10℃ / min, kept constant at 800℃ for 6h, and the cooling rate is controlled to be 5℃ / min. The material is taken out after naturally cooling to 100℃; after cooling to room temperature, it is crushed, sieved, and demagnetized to obtain the second-burned product.
[0073] S3. Mix all the above-prepared second-burned products with Li2CO3, TiO2 and B2O3, wherein the molar ratio of the Li element in Li2CO3 to the total molar number of the metal elements in the precursor is 0.03:1, and the molar ratio of the Ti element in TiO2, the B element in B2O3 and the total molar number of the metal elements in the precursor is 0.0005:0.0010:1. Then, calcinate for the third time in an atmosphere furnace, without ventilation in the heating section and the constant temperature section, and with oxygen in the cooling section. The temperature is raised from room temperature to 400°C at a heating rate of 8°C / min, and maintained at 400°C for 3h. The pressure difference in the furnace is controlled by the furnace head exhaust fan to a pressure difference of 3±2Pa in the cooling section, to obtain Li 1.01 Ni 0.90 Co 0.05 Mn 0.05 Al 0.00192 Y 0.0009 Ti 0.0005 B 0.001 O2 single crystal positive electrode material.
[0074] Example 3
[0075] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0076] S1. Follow step S1 in Example 1, except that the molar ratio of the Li element in LiOH to the total molar number of the metal elements in the precursor is 0.95:1.
[0077] S2. The process is carried out according to step S2 in Example 1, except that the molar ratio of the Li element in LiOH to the total molar number of the metal elements in the precursor is 0.03:1.
[0078] S3. The process is carried out according to step S3 in Example 1, except that the molar ratio of the Li element in LiOH to the total molar number of the metal elements in the precursor is 0.04:1.
[0079] Example 4
[0080] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0081] S1. Follow the steps S1 in Example 1, except that the precursor
[0082] Ni 0.95 Co 0.03 Mn 0.02 (OH)2 is mixed with LiOH and ZrO2, wherein the molar ratio of the Li element in LiOH to the total molar number of the metal elements in the precursor is 0.98:1, and the molar ratio of the Zr element in ZrO2 to the total molar number of the metal elements in the precursor is 0.00192:1;
[0083] S2, following step S2 in Example 1;
[0084] S3. According to step S3 in Example 1, the difference is that all the above-prepared di-sintered products are mixed with LiOH and ZrO2, wherein the molar ratio of the Li element in LiOH to the total molar number of metal elements in the precursor is 0.005:1, and the molar ratio of the Zr element in ZrO2 to the total molar number of metal elements in the precursor is 0.00092:1.
[0085] Example 5
[0086] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0087] S1. Follow the S1 step in Example 1, except that the temperature is raised from room temperature to 720°C at a rate of 2°C / min, maintained at 720°C for 12 hours, and then cooled naturally.
[0088] S2. Follow step S2 in Example 1.
[0089] S3. Follow step S3 in Example 1.
[0090] Example 6
[0091] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0092] S1. Follow the steps S1 in Example 2, except that the precursor
[0093] Ni 0.95 Co 0.03 Mn 0.02 (OH)2 is mixed with Li2CO3, Y2O3, Co3O4 and ZrO2, the molar ratio of Li element in Li2CO3 to the total molar number of metal elements in the precursor is 0.92:1, and the molar ratio of Y element in Y2O3, Co element in Co3O4, Zr element in ZrO2 and the total molar number of metal elements in the precursor is 0.0010:0.00025:0.00067:1.
[0094] S2. Follow step S2 in Example 2.
[0095] S3. Follow step S3 in Example 2.
[0096] Example 7
[0097] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0098] S1. Follow the S1 step in Example 1, except that the molar ratio of the Sr element in SrCO3, the W element in W2O3, the Zr element in ZrO2, and the total molar number of the metal element in the precursor is 0.0020:0.0010:0.0020:1.
[0099] S2. Follow step S2 in Example 1.
[0100] S3. Follow step S3 in Example 1.
[0101] Example 8
[0102] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0103] S1. Follow step S1 in Example 1.
[0104] S2. Follow the S2 step in Example 1, except that the temperature is raised from room temperature to 820°C at a rate of 15°C / min, maintained at 820°C for 8h, the cooling rate is controlled at 3°C / min, and the material is taken out after naturally cooling to 100°C.
[0105] S3. Follow step S3 in Example 1.
[0106] Example 9
[0107] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0108] S1. Follow step S1 in Example 2.
[0109] S2. Follow the S2 step in Example 2, except that all the above-prepared sintered products are mixed with Li2CO3 and Al2O3, wherein the total molar ratio of the Li element in Li2CO3 to the total molar ratio of the metal element in the precursor is 0.06:1, and the molar ratio of the Al element in Al2O3 to the total molar ratio of the metal element in the precursor is 0.0009:1.
[0110] S3. Follow step S3 in Example 2.
[0111] Example 10
[0112] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0113] S1. Follow step S1 in Example 1.
[0114] S2. Follow step S2 in Example 1, except that the molar ratio of the Zr element in ZrO2 to the total molar number of metal elements in the precursor is 0.003:1.
[0115] S3. Follow step S3 in Example 1.
[0116] Embodiment 11
[0117] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0118] S1. Follow step S1 in Example 1.
[0119] S2. Follow step S2 in Example 1.
[0120] S3. Follow the S3 step in Example 1, except that the temperature is increased from room temperature to 650°C at a heating rate of 10°C / min and maintained at 650°C for 3h.
[0121] Example 12
[0122] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0123] S1. Follow step S1 in Example 2.
[0124] S2. Follow step S2 in Example 2.
[0125] S3. Follow the S3 step in Example 2, except that all the above-prepared second-burned products are mixed with Li2CO3, H3BO3, and Al2O3, wherein the molar ratio of the Li element in Li2CO3 to the total molar number of metal elements in the precursor is 0.03:1, and the molar ratio of the B element in H3BO3, the Al element in Al2O3, and the total molar number of metal elements in the precursor is 0.0005:0.0010:1.
[0126] Embodiment 13
[0127] This embodiment provides a method for preparing a single crystal positive electrode material, which is as follows:
[0128] S1. Follow step S1 in Example 1.
[0129] S2. Follow step S2 in Example 1.
[0130] S3. Follow the S3 step in Example 1, except that the molar ratio of the total molar number of the W element in W2O3, the Zr element in ZrO2, and the metal element in the precursor is 0.0005:0.0005:1.
[0131] Comparative Example 1
[0132] This comparative example provides a method for preparing a positive electrode material, which is as follows:
[0133] The average particle size is 2.5 μm and the BET is 15 μm.2 / g, TD is 1.5g / cm 3 , the porosity of the precursor Ni is 35% 0.95 Co 0.03 Mn 0.02 (OH)2 is mixed with LiOH, SrCO3, W2O3 and ZrO2, the molar ratio of Li element in LiOH to the total molar number of metal elements in the precursor is 1.035:1, the molar ratio of Sr element in SrCO3, W element in W2O3, Zr element in ZrO2 and the total molar number of metal elements in the precursor is 0.0010:0.0005:0.0020:1; the mixed powder is calcined in an atmosphere roller kiln, the atmosphere is non-ventilated in the heating section, air in the constant temperature section, and oxygen in the cooling section. The pressure difference in the heating section is ensured by the furnace top gate valve and the furnace head exhaust fan to be -6±2Pa in the heating section, 0±2Pa in the constant temperature section, and 5±2Pa in the cooling section. The temperature was raised from room temperature to 750°C at 9°C / min, kept constant at 750°C for 8 hours, and the cooling rate was controlled at 2.5°C / min. The material was taken out after naturally cooling to room temperature. After that, it was crushed, sieved, and demagnetized to obtain the positive electrode material.
[0134] The morphology of the cathode material is Figure 7 As shown, from Figure 7 It can be seen that the primary particles are in a state of agglomeration, the grain boundaries are not clear, the surface is not smooth, the particle size is not uniform, and they cannot be separated later and cannot grow in the form of single crystals, and ultimately single crystals cannot be obtained.
[0135] Comparative Example 2
[0136] This comparative example provides a method for preparing a positive electrode material, which is as follows:
[0137] S1, the average particle size is 2.5μm, BET is 15m 2 / g, TD is 1.5g / cm 3 , porosity is 35% of the precursor Ni 0.95 Co 0.03 Mn 0.02(OH)2 is mixed with LiOH, SrCO3, W2O3 and ZrO2, wherein the molar ratio of the Li element in LiOH to the total molar number of the metal elements in the precursor is 1.030:1, and the molar ratio of the Sr element in SrCO3, the W element in W2O3, the Zr element in ZrO2 and the total molar number of the metal elements in the precursor is 0.0010:0.00025:0.00013:1; the mixed powder is first heated in an atmosphere roller kiln The first calcination is carried out, with no ventilation in the heating section, air in the constant temperature section, and oxygen in the cooling section. The pressure difference in the heating section is ensured by the furnace top plug valve and the furnace head exhaust fan to be -6±2Pa in the heating section, 0±2Pa in the constant temperature section, and 5±2Pa in the cooling section. The temperature is raised from room temperature to 750°C at 9°C / min, and kept constant at 750°C for 8h. The cooling rate is controlled to be 2.5°C / min. The material is taken out after naturally cooling to 150°C; then it is crushed, sieved, and demagnetized to obtain a calcined product.
[0138] S2, all the above-prepared calcined products are mixed with LiOH, ZrO2, and W2O3, wherein the molar ratio of the Li element in LiOH to the total molar number of the metal elements in the precursor is 0.005:1, and the molar ratio of the W element in W2O3, the Zr element in ZrO2, and the total molar number of the metal elements in the precursor is 0.00025:0.00067:1, and then a second calcination is carried out in an atmosphere furnace, the heating section and the constant temperature section are not ventilated, and oxygen is passed through the cooling section, the temperature is raised from room temperature to 550°C at a heating rate of 8°C / min, and the temperature is kept constant at 550°C for 4h, and the pressure difference in the furnace is controlled by the furnace head exhaust fan to be 3±2Pa in the cooling section, to obtain a positive electrode material;
[0139] The morphology of the cathode material is Figure 8 As shown, from Figure 8 It can be seen that the primary particles are in a state of agglomeration, the grain boundaries are not clear, they cannot be separated later, and cannot grow in the form of single crystals.
[0140] Comparison column 3
[0141] This comparative example provides a method for preparing a single crystal positive electrode material, which is as follows:
[0142] S1. Follow step S1 in Example 1.
[0143] S2. Follow step S2 in Example 1.
[0144] S3. Follow the S3 step in Example 1, except that air is passed through the temperature rising section, constant temperature section and temperature falling section.
[0145] Comparative Example 4
[0146] This comparative example provides a method for preparing a positive electrode material, which is as follows:
[0147] S1. Follow the S1 step in Example 1, except that the pressure difference in the furnace is maintained at -30±2Pa.
[0148] S2. Follow the S2 step in Example 1, except that the pressure difference in the temperature rising section is -15±2Pa, the pressure difference in the constant temperature section is -8±2Pa, and the pressure difference in the temperature falling section is -3±2Pa.
[0149] S3. Follow the S3 step in Example 1, except that the pressure difference in the furnace is controlled by the furnace head exhaust fan to a pressure difference of 1±2Pa in the temperature reduction section.
[0150] The LiOH content and Li2CO3 content of the positive electrode material were obtained by potentiometric titration.
[0151] Prepared into batteries: The preparation of positive electrode sheets mainly includes pulping, coating, drying, and tableting. Pulping refers to preparing the powdered positive electrode material into a slurry. The positive electrode material: conductive agent (acetylene black): binder (polyvinylidene fluoride, PVDF) = 95:2.5:2.5 is stirred and mixed evenly on a magnetic stirrer, and then N-methylpyrrolidone (NMP) is added. The ratio of positive electrode material to NMP is 4:9g / mL, and stirring is continued for 30 minutes. Use a scraper to evenly coat the slurry on one side with a scraper of 400μm. After coating, it is blown and vacuum dried to remove the solvent NMP and moisture. The drying temperature is 120℃ and the drying time is 8h. After coating, a roller press is used to press the sheet, and the thickness of the electrode sheet is controlled to be 50μm. It is cut into discs with a diameter of 13mm, and the compaction density is maintained at 2.0g / cm 3 .
[0152] Assembly of button cell
[0153] The button half-cell is assembled in a glove box filled with argon, with a water content of less than 0.5ppm. The specific components of the electrolyte are ethylene carbonate (EC) and diethyl carbonate (DEC), and the volume ratio of EC to DEC is 1:1. The order of assembling the battery is negative electrode shell-gasket-electrolyte-lithium sheet (Ф16mm)-electrolyte-diaphragm (Ф19mm)-electrolyte-positive electrode sheet-gasket-positive electrode shell. Finally, press it for use.
[0154] After standing for 6 hours, the temperature was controlled at 25°C, and the battery was charged to 4.4V at a constant current rate of 0.1C, and then discharged to 3.0V at a rate of 0.1C. The calculation formula is: specific capacity = 0.1C first cycle discharge capacity / mass × 100%.
[0155] After standing for 6 hours, the temperature was controlled to 25°C, and the battery was charged to 4.4V at a constant current rate of 0.1C, and then discharged to 3.0V at a rate of 0.1C, and repeated 50 times. The discharge capacity at the first cycle and the discharge capacity at the 50th cycle were measured, and the cycle capacity retention rate was calculated; the temperature was then controlled to 60°C, and the battery was charged to 4.4V at a constant current rate of 0.1C, and then discharged to 3.0V at a rate of 0.1C, and repeated 50 times. The discharge capacity at the first cycle and the discharge capacity at the 50th cycle were measured, and the cycle capacity retention rate was calculated. The calculation formula is: 50-cycle cycle capacity retention rate = discharge capacity at the 50th cycle / discharge capacity at the first cycle × 100%; The battery containing the prepared positive electrode material was tested, and the specific results are shown in Table 1.
[0156] Table 1
[0157]
[0158]
[0159] By comparing the embodiment with the comparative example, it can be seen that the residual alkali content on the surface of the positive electrode material in the embodiment is lower, and the battery after being manufactured has better battery capacity and cycle performance.
[0160] Figure 5 This is the first cycle charge and discharge capacity curve of Example 1. It can be seen from the figure that the charging capacity is 237.0mAh / g and the discharge capacity is 216.0mAh / g, which has exceeded the discharge capacity of conventional 9 series single crystal material batteries in the market. The discharge capacity of conventional 9 series single crystal material batteries is 200.0-210.0mAh / g.
[0161] Figure 6 It is the capacity retention rate after 50 cycles of Example 1. It can be seen from the figure that the 25°C cycle retention rate is 97.0%, which has exceeded the cycle retention rate of conventional 9-series single crystal material batteries in the market. The cycle retention rate of conventional 9-series single crystal material batteries is 90.0-95.0%.
[0162] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a single crystal positive electrode material, characterized in that: The preparation steps include: S1, mixing a precursor, a first lithium source, and a first additive, wherein the ratio of the total molar number of lithium element in the first lithium source to the total molar number of metal element in the precursor is a:1, 0.9<a<1.0, and performing a first calcination to obtain a calcined product; Among them, the temperature rising section, constant temperature section and temperature falling section of the first calcination are ventilated with air; the pressure difference in the furnace is -20 to -3Pa; S2, mixing the first calcined product, the second lithium source, and the second additive, wherein the ratio of the total molar number of the lithium element in the second lithium source to the total molar number of the metal element in the first calcined product is a':1, 0<a'≤0.06, and performing a second calcination to obtain a second calcined product; The second calcination has no ventilation in the heating section, air in the constant temperature section, and oxygen in the cooling section; the pressure difference in the furnace in the heating section is -12 to -3Pa, the pressure difference in the furnace in the constant temperature section is -5 to 3Pa, and the pressure difference in the furnace in the cooling section is 0-10Pa; S3, mixing the second calcined product, the third lithium source, and the third additive, wherein the ratio of the total molar number of the lithium element in the third lithium source to the total molar number of the metal element in the second calcined product is 0<a″≤0.05, and performing a third calcination to obtain a single crystal positive electrode material; Among them, the temperature rising section and constant temperature section of the third calcination are not ventilated, and oxygen is ventilated in the temperature dropping section; the pressure difference in the furnace in the temperature dropping section is 1-5Pa.
2. The preparation method according to claim 1, characterized in that: The average particle size of the precursor is 1-5 μm, and the specific surface area is 10-20 m 2 / g, tap density is 1.2-1.8g / cm 3 , the porosity is 30-40%.
3. The preparation method according to claim 1 or 2, characterized in that: The specific conditions of the first calcination are as follows: a heating rate of 2-6°C / min, a constant temperature of 630-730°C, and a constant temperature time of 6-12h.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The total molar ratio of the metal element in the first additive to the metal element in the precursor is 0.0010-0.0050:1; Optionally, the first additive includes at least one of metal oxides, metal carbonate compounds, and metal hydroxides, and can be any one of SrCO3, W2O3, ZrO2, Y2O3, Al2O3, Al(OH)3, and Co3O4.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The specific conditions of the second calcination are as follows: the heating rate is 8-16°C / min, the constant temperature is 730-830°C, and the constant temperature time is 6-12h; the cooling rate is 2-6°C / min, and the material is taken out when the temperature drops to 100-200°C.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The total molar ratio of the metal element in the second additive to the metal element in the precursor is 0.0005-0.0050:1; Optionally, the second additive includes metal oxide and / or metal hydroxide, which can be any one of ZrO2, TiO2, Y2O3, Al2O3, Al(OH)3, and Co3O4.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The specific conditions of the third calcination are as follows: a heating rate of 5-10° C. / min, a constant temperature of 400-700° C., and a constant temperature time of 2-6 h.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The total molar ratio of the metal element in the third additive to the metal element in the precursor is 0.0005-0.0020:
1.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The third additive includes at least one of boric acid, oxides, and metal hydroxides, and can be selected from any one of W2O3, ZrO2, TiO2, Y2O3, Al2O3, Al(OH)3, H3BO3, and B2O3.
10. A single crystal positive electrode material obtained by the preparation method according to any one of claims 1 to 9, characterized in that: The positive electrode material is generally Li a+a’+a” Ni x Co y Mn z M b O2; Among them, 0.9 <a M is at least one of Zr, Sr, W, Ti, Y, Co, Al, and B.