Armored aerogel fiber as well as preparation method and application thereof
By forming a dense heat-shrinkable material shell on the aerogel fiber, the problems of large evaporation resistance and poor mechanical strength caused by its loose porous structure are solved, and the long-distance anti-gravity transportation and high-strength effects of liquids are achieved.
Patent Information
- Application Number
- CN202411410142.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to realize the lossless packaging of aerogel fibers, and its loose porous outer wall leads to large evaporation resistance, making it impossible to achieve long-distance anti-gravity transportation of liquids, and has poor mechanical strength, which cannot meet the actual application needs.
Armored aerogel fiber adopting a coaxial structure, the inner layer is aerogel fiber material with a continuous three-dimensional multi-stage pore network structure, and the outer layer is a dense heat-shrinkable material. The heat-shrinkable material is shrinked and clamped by heating. The outer wall of the aerogel fiber forms a dense and tough shell.
It realizes the dense and tough shell of aerogel fiber, reduces evaporation resistance, improves mechanical strength and moisture resistance, and can realize long-distance anti-gravity transportation of liquids, meeting application needs in the fields of textiles, microfluidics, etc.
Smart Images

Figure CN119061513A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aerogel and fluid control, in particular to the technical field of armoring of aerogel fibers, and specifically to an armored aerogel fiber, a preparation method of the armored aerogel fiber and applications thereof. Background Art
[0002] The spontaneous rise of water in tall trees continues to attract scientists because it can overcome gravity without the help of energy-intensive tanks, pumps or valves. Self-driven anti-gravity liquid transport devices are of great significance in industrial activities such as microfluidics, seawater desalination and water-saving irrigation. Trees can transport water from the ground to the crown over vertical distances of even more than 100 m. This anti-gravity transport ability depends on their complex porous system (with high capillary driving force and low flow resistance) and relatively dense bark (with low evaporation resistance) and transpiration (providing negative pressure) to maximize the driving force of anti-gravity transport and minimize the transport resistance.
[0003] Aerogels have rich mesoporous structures that can provide strong capillary driving forces and are highly favored in the field of anti-gravity liquid transport. Xu et al. (Xu, W., et al., ACS Nano, 2019.13: p.7930-7938.) designed a double-layer aerogel with excellent capillary rise performance, which achieved long-distance (28 cm rise in 190 min) anti-gravity water transport on a macro scale. However, due to the collapse of the mesoporous structure during freeze-drying, the capillary driving force is insufficient, and the loose porous surface structure leads to a large evaporation resistance, which causes the anti-gravity water transport height of the aerogel to be low.
[0004] Aerogel fiber is a new type of functional fiber material that combines the light weight and multi-mesoporous properties of aerogel with the flexibility and slenderness of fiber. Compared with traditional block aerogel materials, aerogel fibers have excellent reprocessability and flexibility. Compared with traditional fiber materials, aerogel fibers have ultra-high porosity and specific surface area. Based on the unique properties of aerogel fibers, it has broad application prospects in the fields of smart fabrics, flexible electronic devices, thermal insulation fibers and microfluidics. Aerogel fibers, which have rich mesoporous structures, have a strong capillary driving force for liquids, especially mesoporous aerogel fibers, are ideal materials for realizing long-distance anti-gravity transport of liquids. However, in the practice of anti-gravity liquid transport, technicians in this field have found that the loose and porous outer wall of aerogel fibers will lead to a large evaporation resistance, making it impossible to realize long-distance anti-gravity transport of liquids. In addition, due to the porous skeleton structure of aerogel fibers, the mechanical strength is poor, the brittleness is large, and other reasons cannot meet the needs of practical applications. The prior art has attempted to encapsulate aerogel fibers in order to improve their mechanical properties. Patent CN 117328156A reports a method of immersing the aerogel fibers in an encapsulation solution to encapsulate a dense polymer layer on the surface of the aerogel fibers to improve their mechanical strength. Specifically, the aerogel fibers are immersed in a polymer solution, and the solvent in the polymer solution is evaporated by high-temperature drying to form a dense polymer encapsulation layer on the surface of the aerogel fibers. In addition, patent CN116376267 A also reports a method of immersing aerogel in an encapsulation solution to obtain an encapsulated aerogel material. The above-mentioned methods of encapsulating aerogel fibers or aerogels all use a method of immersing them in an encapsulation solution. Due to the strong capillary force of the aerogel, the encapsulation solution can easily enter the porous network, causing damage to the mesoporous structure, and the operation is relatively complicated. Therefore, there is an urgent need for an encapsulation method that is simple and easy to operate and does not damage the mesoporous structure of the aerogel.
[0005] In summary, there is currently no technology that can achieve lossless encapsulation of aerogel fibers, and in some application fields of aerogel fibers, especially in the field of anti-gravity liquid transportation, encapsulation of aerogel fibers is important and valuable. Summary of the invention
[0006] The main purpose of the present invention is to provide an armored aerogel fiber and a preparation method thereof to overcome the deficiencies in the prior art.
[0007] Another object of the present invention is to provide applications of the armored aerogel fiber.
[0008] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: An embodiment of the present invention provides an armored aerogel fiber, which includes: an inner layer and an outer layer in a coaxial structure, the outer layer is tightly fitted to the outer wall of the inner layer, the inner layer includes an aerogel fiber material with a continuous three-dimensional multi-level pore network structure, and the outer layer includes a dense heat-shrinkable material.
[0009] An embodiment of the present invention also provides a method for preparing an armored aerogel fiber, which includes: inserting the aerogel fiber into a heat-shrinkable material, heating it to the shrinkage temperature of the heat-shrinkable material, causing the heat-shrinkable material to shrink and adhere to the outer wall of the aerogel fiber, and obtaining the armored aerogel fiber.
[0010] The embodiment of the present invention also provides armored aerogel fiber prepared by the above-mentioned preparation method.
[0011] The embodiments of the present invention also provide applications of the armored aerogel fiber in the fields of anti-gravity liquid transport, thermal management, smart fabrics, wearable devices, environmental management, sensing, sound absorption and noise reduction, thermal insulation, optics, textiles or microfluidics.
[0012] Compared with the prior art, the beneficial effects of the present invention include at least: 1) Compared with unarmored aerogel fibers, the armored aerogel fibers provided by the present invention have a dense and tough shell, thus having excellent mechanical strength and moisture resistance; at the same time, the dense outer wall leads to a small evaporation resistance, which has great advantages in the field of anti-gravity liquid transportation and can realize long-distance anti-gravity transportation of liquids; 2) Compared with the traditional preparation method of immersing in encapsulation solution, the preparation method of the armored aerogel fiber provided by the present invention has the advantages of being simple and easy to operate and having no damage to the aerogel mesoporous structure. The aerogel does not need to undergo the solvent wetting-drying process again, and can completely maintain its three-dimensional network skeleton structure. The obtained armored aerogel fiber can meet practical applications, such as application in textile and microfluidics fields.
[0013] 3) The preparation method of the armored aerogel fiber provided by the present invention fills the gap in the lossless armor technology of aerogel fibers, and promotes the practical application of aerogel fibers in pipeline drag reduction, thermal management, smart fabrics, wearable devices, environmental governance, sensing, sound absorption and noise reduction, thermal insulation, optics and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1 is a scanning electron microscope photograph of a cross section of an armored aerogel fiber in a typical embodiment of the present invention; Figure 2 This is a digital photo comparing the aerogel fibers before and after armoring obtained in Example 1 of the present invention; Figure 3 is a scanning electron microscope photograph of the cross section of the armored aerogel fiber obtained in Example 1 of the present invention; Figure 4 is a nitrogen adsorption-desorption curve diagram of the armored aerogel fiber obtained in Example 2 of the present invention; Figure 5 is a pore size distribution diagram of the armored aerogel fiber obtained in Example 2 of the present invention; Figure 6 is a tensile stress-strain curve diagram of the armored aerogel fiber obtained in Example 3 of the present invention; Figure 7 This is a thermal gravimetric curve of the armored aerogel fiber obtained in Example 4 of the present invention.
[0016] Figure 8 This is a digital photo comparing the aerogel fibers before and after armoring obtained in Comparative Example 1 of the present invention.
[0017] Fig. 9 This is a digital photo comparing the aerogel fibers before and after armoring obtained in Comparative Example 2 of the present invention.
[0018] Fig.10 This is a digital photo comparing the aerogel fibers before and after armoring obtained in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0019] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice, which mainly provides a method for preparing armored aerogel fibers and their application in anti-gravity liquid transportation, filling the gap in the technology of lossless armoring of aerogel fibers, aiming to solve the thorny problems in the prior art of immersing aerogel fibers in armoring solutions, such as the easy destruction of their mesoporous structure and the collapse of the three-dimensional network. The technical solution, its implementation process and principle will be further explained as follows.
[0020] As one aspect of the technical solution of the present invention, an armored aerogel fiber involved therein comprises: an inner layer and an outer layer in a coaxial structure, the outer layer being tightly fitted to the outer wall of the inner layer, the inner layer comprising an aerogel fiber material having a continuous three-dimensional multi-level pore network structure, and the outer layer comprising a dense heat-shrinkable material.
[0021] In some embodiments, the heat-shrinkable material is a heat-shrinkable plastic material, for example, it may specifically include any one or a combination of two or more of polyvinyl chloride (PVC) heat shrinkable tube, polyethylene (PE) heat shrinkable tube, polyethylene terephthalate (PET) heat shrinkable tube, ethylene-vinyl acetate copolymer (EVA) heat shrinkable tube, glue-containing double-wall heat shrinkable tube, imitation wood grain heat shrinkable tube, polyolefin (PO) heat shrinkable tube, cross-linked polyolefin heat shrinkable tube, polytetrafluoroethylene (PTFE) heat shrinkable tube, fluorinated ethylene propylene (FEP) heat shrinkable tube, perfluoroalkoxy resin (PFA) heat shrinkable tube, polyvinylidene fluoride (PVDF) heat shrinkable tube, etc., but is not limited to these.
[0022] In some embodiments, the shrinkage ratio of the heat shrinkable material is 1:1 to 6:1.
[0023] In some embodiments, the shrinkage temperature of the heat shrinkable material is 50°C to 600°C.
[0024] In some embodiments, see Figure 1 As shown, the armored aerogel fiber is composed of two inner and outer layers in a coaxial structure, wherein the inner layer is composed of an aerogel fiber material having a continuous three-dimensional multi-level pore network structure, and the outer layer is composed of a dense heat-shrinkable plastic material.
[0025] In some embodiments, the three-dimensional multi-level porous network structure includes micropores with a pore size of less than 2 nm, mesopores with a pore size of 2 to 50 nm, and macropores with a pore size of 50 nm to 100 nm.
[0026] Furthermore, the density of the aerogel fiber material of the inner layer is 0.001 to 1 g / cm 3 The porosity is 1.0-99.9%, and the specific surface area is 1-1000 m 2 / g.
[0027] In some embodiments, the material of the inner layer of aerogel fiber material includes any one or a combination of two or more of aromatic polyamide, chitosan, sodium alginate, graphene, MXene, cellulose, silk fibroin, silicon oxide, polyimide, carbon nanotubes, boron nitride, carbon aerogel, etc., but is not limited thereto.
[0028] In some embodiments, the aerogel fiber material of the inner layer includes any one or a combination of two of medium-sized aerogel fibers and non-medium-sized aerogel fibers.
[0029] In some embodiments, the inner layer has a diameter of 0.001 to 100 mm.
[0030] In some embodiments, the outer layer has a diameter of 0.002 to 100 mm.
[0031] In some embodiments, the thickness ratio of the inner layer of aerogel fiber material to the outer layer of heat shrinkable material is 2000:1 to 1:1000.
[0032] In some embodiments, the armored aerogel fiber has a tensile strength of 10 to 3000 MPa and an elongation at break of 1 to 3000%.
[0033] Furthermore, the armored aerogel fiber has a dense and tough plastic outer layer and a high-porosity aerogel inner layer. The dense and tough plastic outer layer can make the armored aerogel fiber have excellent mechanical strength and moisture resistance. In addition, the dense outer wall will lead to a small evaporation resistance, which has great advantages in the field of anti-gravity liquid transportation, and can achieve long-distance anti-gravity transportation of liquids, solving the problem that the outer wall of aerogel and / or aerogel fiber is loose and porous, resulting in a large evaporation resistance, thereby failing to achieve long-distance anti-gravity transportation of liquids.
[0034] As another aspect of the technical solution of the present invention, a method for preparing an armored aerogel fiber involves: sheathing the aerogel fiber in a heat-shrinkable material, heating it to the shrinkage temperature of the heat-shrinkable material, causing the heat-shrinkable material to shrink and adhere to the outer wall of the aerogel fiber, and obtaining the armored aerogel fiber.
[0035] The specific types of heat-shrinkable materials used in the preparation method are as described above and will not be repeated here.
[0036] In some embodiments, the shrinkage ratio of the heat shrinkable material is 1:1 to 6:1.
[0037] In some embodiments, the shrinkage temperature of the heat shrinkable material is 50°C to 600°C, that is, the heat shrinkable material is heated to 30°C to 600°C to shrink and adhere to the outer wall of the aerogel fiber.
[0038] In some embodiments, the diameter of the heat shrinkable material is 0.002-100 mm.
[0039] In some embodiments, the heating shrinkage time is 1s to 6h.
[0040] In some embodiments, the preparation method comprises: The spinning solution is subjected to a spinning technique to obtain a wet gel fiber; The wet gel fiber is dried to obtain aerogel fiber.
[0041] In some more specific embodiments, the method for preparing the armored aerogel fiber comprises: Firstly, the spinning solution is subjected to spinning technology to obtain wet gel fiber; Then the wet gel fiber is dried to obtain aerogel fiber; Finally, the aerogel fiber is armored with a heat shrink tube to obtain armored aerogel fiber.
[0042] In some embodiments, the spinning solution may include any one or a combination of two or more of an aromatic polyamide nanofiber dispersion, an aromatic polyamide molecule solution, a chitosan solution, a sodium alginate solution, a graphene oxide dispersion, a MXene dispersion, a cellulose nanofiber dispersion, a cellulose nanocrystal solution, a silk fibroin solution, a silica sol, a polyimide precursor solution, a carbon nanotube dispersion, a boron nitride precursor solution, a carbon precursor solution, etc., but is not limited thereto.
[0043] In some embodiments, the spinning technology includes any one or a combination of two or more of gel spinning technology, wet spinning technology, dry spinning technology, dry-jet wet spinning technology, dry-freeze spinning technology, 3D printing technology, mold filamentation technology, coaxial wet spinning technology, coaxial 3D printing technology, coaxial dry-freeze spinning technology, etc. Furthermore, the spinning technology can preferably be any one or a combination of two of wet spinning technology and coaxial wet spinning technology.
[0044] Furthermore, the wet spinning technology includes: providing a spinning solution of a selected concentration, extruding the spinning solution into a coagulation bath through a spinneret or a spinning needle to form a wet gel fiber; wherein the process conditions adopted by the wet spinning technology include: the concentration of the spinning solution is 0.1 to 20 wt%, the diameter of the spinning needle is 10 to 5000 μm, and the extrusion speed is 5 to 5000 μL / min.
[0045] Furthermore, the coaxial wet spinning technology includes: providing a first spinning solution (also referred to as "spinning solution A") of a selected concentration, using a selected solvent as a second spinning solution (also referred to as "spinning solution B"), and simultaneously extruding the first spinning solution (i.e., spinning solution A) and the second spinning solution (i.e., spinning solution B) into a coagulation bath through a hollow spinneret or a coaxial needle to obtain wet gel fiber; wherein the process conditions adopted by the coaxial wet spinning technology include: the concentration of the first spinning solution is 0.1 to 20wt%, the extrusion speed of the first spinning solution (i.e., spinning solution A) is 5 to 5000 μL / min, and the extrusion speed of the second spinning solution (i.e., spinning solution B) is 5 to 5000 μL / min.
[0046] Furthermore, the selected solvent includes any one or a combination of two or more of water, metal ion aqueous solution, acid solution, alkaline solution, and organic solvent, but is not limited thereto.
[0047] Furthermore, the inner needle model of the coaxial needle is 10G-30G, and the outer needle model of the coaxial needle is 8G-28G.
[0048] In some more specific embodiments, the coagulation bath used in the wet spinning technology and the coaxial wet spinning technology includes a main component and an auxiliary component. The main component includes any one or a combination of two or more of water, ethanol, acetone, acetic acid, dimethyl sulfoxide, nitrogen methyl pyrrolidone, ethyl acetate, dimethyl silicone oil, N, N-dimethylformamide, etc.; the auxiliary component includes any one or a combination of two or more of sulfuric acid, hydrochloric acid, ascorbic acid, calcium chloride, ferric chloride, potassium hydroxide, sodium hydroxide, ammonium hydroxide, etc., but is not limited thereto.
[0049] Furthermore, the mass ratio of the main component to the auxiliary component is 1:0~1:99.
[0050] In some more specific embodiments, the preparation method includes: first replacing the non-drying solvent in the wet gel fiber with an easy-drying solvent, and then drying the replaced wet gel fiber. The easy-drying solvent can include any one or a combination of two or more of water, methanol, ethanol, tert-butanol, hexafluoroisopropanol, acetone, cyclohexane and n-hexane, but is not limited to these.
[0051] Furthermore, the drying process includes any one or a combination of two or more of supercritical fluid drying, vacuum freeze drying, reduced pressure drying and normal pressure drying, but is not limited thereto.
[0052] In summary, compared with the previous preparation method of immersing in armoring solution, the preparation method of armored aerogel fiber provided by the present invention has the advantages of being simple and easy to operate and having no damage to the aerogel mesoporous structure. The aerogel does not need to go through the solvent wetting-drying process again, and its three-dimensional network skeleton structure can be completely maintained. The armored aerogel fiber obtained can meet practical applications, such as in the fields of textiles and microfluidics.
[0053] As another aspect of the technical solution of the present invention, it also relates to armored aerogel fibers prepared by the aforementioned preparation method.
[0054] As another aspect of the technical solution of the present invention, it also relates to the application of the armored aerogel fiber in anti-gravity liquid transportation.
[0055] Furthermore, the preparation method of the armored aerogel fiber provided by the present invention fills the gap in the lossless armoring technology of aerogel fibers, and promotes the practical application of aerogel fibers in pipeline drag reduction, human thermal management, smart fabrics, wearable devices, environmental governance, sensing, sound absorption and noise reduction, thermal insulation, optics, textiles, microfluidics and other fields.
[0056] In summary, through the above technical scheme, the present invention provides a method for preparing armored aerogel fibers, which has simple preparation steps, short time consumption (completed within a few seconds), and does not require harmful substances such as organic solvents that are difficult to recycle, and has moderate cost. The method can be prepared continuously, is simple to operate, is green and environmentally friendly, has moderate cost, is conducive to scale-up and facilitates industrial production, and has good industrialization prospects. The armored aerogel fibers obtained have the characteristics of light weight, high specific surface area, high strength, high flexibility, etc., can be woven and applied to extreme environments or special environments, further expanding the application range of such materials.
[0057] The technical scheme of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, but not to limit the scope of the present invention, and those skilled in the art can adjust according to actual conditions. The implementation conditions adopted in the following examples can be further adjusted according to actual needs, and the implementation conditions not specified are usually the conditions in routine experiments.
[0058] Example 1 (1) A 3.0 wt% aromatic polyamide nanofiber dispersion was used as spinning solution A, and water was used as spinning solution B. The spinning solution A and the spinning solution B were simultaneously extruded into a water coagulation bath at an extrusion rate of 300 μL / min through a coaxial needle (inner 22G-outer 17G) to obtain a hollow aromatic polyamide wet gel fiber.
[0059] (2) The hollow aromatic polyamide wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is ethanol), and then supercritical drying is performed to obtain the hollow aromatic polyamide aerogel fiber.
[0060] (3) The hollow aromatic polyamide aerogel fiber of step (2) is loaded into a polyethylene heat shrinkable tube with a diameter of 1.5 mm and a shrinkage ratio of 2:1, and placed in a 120° C. oven for 15 seconds to shrink the polyethylene heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the hollow aromatic polyamide aerogel fiber to obtain an armored aerogel fiber.
[0061] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 250 μm, the thickness of the outer layer of the heat shrinkable material is 300 μm, the thickness ratio of the inner layer to the outer layer is 5:6, the porosity of the inner layer aerogel fiber material is 99.5%, and the specific surface area is 289 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 14.5 MPa, and the elongation at break is about 800%.
[0062] After the above steps, the armored aerogel fiber obtained in this embodiment is shown in the figure Figure 2 As shown, the scanning electron microscope photograph of the cross section of the armored aerogel fiber obtained in this embodiment is as shown in Figure 3 shown.
[0063] Example 2 (1) A 4.0 wt% aromatic polyamide molecular solution is wet-spinned to obtain aromatic polyamide wet gel fibers, specifically, the 4.0 wt% aromatic polyamide molecular solution is extruded through a spinning needle with a diameter of 500 μm at an extrusion rate of 200 μL / min, and then enters a deionized water coagulation bath to obtain aromatic polyamide wet gel fibers; (2) The aromatic polyamide wet gel fiber prepared in step (1) is subjected to solvent replacement (the easily dry solvent used is tert-butyl alcohol), and then freeze-dried to obtain aromatic polyamide aerogel fiber.
[0064] (3) The aromatic polyamide aerogel fiber prepared in step (2) is loaded into a polyvinyl chloride heat shrinkable tube with a diameter of 1.0 mm and a shrinkage ratio of 3:1, and the tube is placed in an oven at 150° C. for 30 s to shrink the polyvinyl chloride heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the aromatic polyamide aerogel fiber to obtain armored aerogel fiber.
[0065] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 400 μm, the thickness of the outer layer of the heat shrinkable material is 250 μm, the thickness ratio of the inner layer to the outer layer is 8:5, the porosity of the inner layer aerogel fiber material is 99.2%, and the specific surface area is 302 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 18MPa, and the elongation at break is about 450%.
[0066] After the above steps, the nitrogen absorption-desorption curve of the armored aerogel fiber obtained in this embodiment is as follows: Figure 4 As shown, the pore size distribution diagram of the armored aerogel fiber obtained in this embodiment is as follows Figure 5 shown.
[0067] Example 3 (1) A 10.0 wt% MXene dispersion was wet-spinned to obtain MXene wet gel fibers. Specifically, a 10.0 wt% aromatic polyamide molecular solution was extruded through a spinning needle with a diameter of 300 μm at an extrusion rate of 100 μL / min and then entered into a calcium chloride aqueous solution coagulation bath to obtain MXene wet gel fibers; (2) After solvent replacement (the easily dry solvent used is acetone) of the MXene wet gel fiber in step (1), MXene aerogel fiber is obtained by supercritical drying.
[0068] (3) The MXene aerogel fiber prepared in step (2) is placed in a polyethylene terephthalate (PET) heat shrink tube with a diameter of 0.5 mm and a shrinkage ratio of 2:1, and is placed in a 150°C oven for 90 s to shrink the polyethylene terephthalate heat shrink tube. After shrinkage, the inner wall of the heat shrink tube is closely attached to the outer wall of the MXene aerogel fiber to obtain an armored aerogel fiber.
[0069] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 250 μm, the thickness of the outer layer of the heat shrinkable material is 200 μm, the thickness ratio of the inner layer to the outer layer is 5:4, the porosity of the inner layer aerogel fiber material is 98%, and the specific surface area is 101 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 21MPa, and the elongation at break is about 1100%.
[0070] After the above steps, the tensile stress-strain curve of the armored aerogel fiber obtained in this embodiment is as follows: Figure 6 shown.
[0071] Example 4 (1) A 2.0 wt% aromatic polyamide nanofiber dispersion was used as spinning solution A, and ethanol was used as spinning solution B. The spinning solution A and the spinning solution B were simultaneously extruded into an ethanol coagulation bath through a coaxial needle (15G inside and 10G outside) at an extrusion rate of 800 μL / min to obtain a hollow aromatic polyamide wet gel fiber.
[0072] (2) The hollow aromatic polyamide wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is acetone), and then supercritical drying is performed to obtain the hollow aromatic polyamide aerogel fiber.
[0073] (3) The hollow aromatic polyamide aerogel fiber of step (2) is loaded into a polytetrafluoroethylene heat shrinkable tube with a diameter of 2.5 mm and a shrinkage ratio of 2:1, and placed in a 400° C. vacuum oven for 3 min to shrink the polytetrafluoroethylene heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the hollow aromatic polyamide aerogel fiber to obtain an armored aerogel fiber.
[0074] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 400 μm, the thickness of the outer layer of the heat shrinkable material is 400 μm, the thickness ratio of the inner layer to the outer layer is 1:1, the porosity of the inner layer aerogel fiber material is 99%, and the specific surface area is 251 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 25.5MPa, and the elongation at break is about 200%.
[0075] After the above steps, the thermal weight loss curve of the armored aerogel fiber obtained in this embodiment is as follows: Figure 7 shown.
[0076] Example 5 (1) a 20.0 wt% sodium alginate solution is wet-spinned to obtain a sodium alginate wet gel fiber, specifically, the 20.0 wt% sodium alginate solution is extruded at an extrusion rate of 300 μL / min through a spinning needle with a diameter of 700 μm and then enters a calcium chloride aqueous solution coagulation bath to obtain a sodium alginate wet gel fiber; (2) The sodium alginate wet gel fiber in step (1) is subjected to solvent replacement (the easily dry solvent used is ethanol), and then supercritical drying is performed to obtain the sodium alginate aerogel fiber.
[0077] (3) The sodium alginate aerogel fiber of step (2) is loaded into a polyolefin (PO) heat shrinkable tube with a diameter of 1.5 mm and a shrinkage ratio of 3:1, and is placed in a 130° C. vacuum oven for 60 s to shrink the polyolefin heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the sodium alginate aerogel fiber to obtain an armored aerogel fiber.
[0078] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 500 μm, the thickness of the outer layer of the heat shrinkable material is 300 μm, the thickness ratio of the inner layer to the outer layer is 5:3, the porosity of the inner layer aerogel fiber material is 92%, and the specific surface area is 189 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 65MPa, and the elongation at break is about 800%.
[0079] Example 6 (1) obtaining graphene oxide wet gel fibers by wet spinning a 15.0 wt% graphene oxide dispersion, specifically, extruding the 15.0 wt% graphene oxide dispersion through a spinning needle with a diameter of 1000 μm at an extrusion rate of 50 μL / min, and then entering a calcium chloride aqueous solution coagulation bath to obtain graphene oxide wet gel fibers, which are further reduced to graphene wet gel fibers; (2) The graphene wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is acetone), and then supercritical drying is performed to obtain graphene aerogel fiber.
[0080] (3) The graphene aerogel fiber of step (2) is loaded into a perfluoroalkoxy resin (PFA) heat shrinkable tube with a diameter of 5 mm and a shrinkage ratio of 6:1, and the perfluoroalkoxy resin heat shrinkable tube is placed in a 350°C oven for 120 s to shrink the perfluoroalkoxy resin heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the graphene aerogel fiber to obtain an armored aerogel fiber.
[0081] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 600 μm, the thickness of the outer layer of the heat shrinkable material is 300 μm, the thickness ratio of the inner layer to the outer layer is 2:1, the porosity of the inner layer aerogel fiber material is 98%, and the specific surface area is 450 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 16MPa, and the elongation at break is about 100%.
[0082] Example 7 (1) a 6.0 wt% cellulose nanofiber dispersion is subjected to a wet spinning method to obtain cellulose wet gel fibers. Specifically, the 6.0 wt% cellulose nanofiber dispersion is extruded through a spinning needle with a diameter of 400 μm at an extrusion rate of 300 μL / min, and then enters a water coagulation bath to obtain cellulose wet gel fibers; (2) The cellulose wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is ethanol), and then supercritical drying is performed to obtain cellulose aerogel fiber.
[0083] (3) The cellulose aerogel fiber of step (2) is loaded into a double-walled heat shrinkable tube containing glue with a diameter of 1 mm and a shrinkage ratio of 3:1, and the double-walled heat shrinkable tube is placed in a 100° C. oven for 180 s to shrink the double-walled heat shrinkable tube containing glue. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the cellulose aerogel fiber to obtain armored aerogel fiber.
[0084] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 350 μm, the thickness of the outer layer of the heat shrinkable material is 300 μm, the thickness ratio of the inner layer to the outer layer is 1.17:1, the porosity of the inner layer aerogel fiber material is 97%, and the specific surface area is 310 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 13.6 MPa, and the elongation at break is about 460%.
[0085] Example 8 (1) A 6.0 wt% chitosan solution was wet-spinned to obtain chitosan wet gel fibers. Specifically, the 6.0 wt% chitosan solution was extruded through a spinning needle with a diameter of 150 μm at an extrusion rate of 200 μL / min and then entered into a potassium hydroxide aqueous solution coagulation bath to obtain chitosan wet gel fibers; (2) The chitosan wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is acetone), and then chitosan aerogel fiber is obtained by supercritical drying.
[0086] (3) The chitosan aerogel fiber prepared in step (2) is placed in a cross-linked polyolefin heat shrinkable tube with a diameter of 1 mm and a shrinkage ratio of 6:1, and placed in a 90°C oven for 300 s to shrink the cross-linked polyolefin heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the chitosan aerogel fiber to obtain armored aerogel fiber.
[0087] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 120 μm, the thickness of the outer layer of the heat shrinkable material is 300 μm, the thickness ratio of the inner layer to the outer layer is 2:5, the porosity of the inner layer aerogel fiber material is 96.5%, and the specific surface area is 190 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 14.5 MPa, and the elongation at break is about 560%.
[0088] Example 9 (1) a 5.0 wt% silica sol solution is wet-spinned to obtain a silica wet gel fiber, specifically, the 5.0 wt% silica sol solution is extruded through a spinning needle with a diameter of 100 μm at an extrusion rate of 1200 μL / min and then enters an ammonia solution coagulation bath to obtain a silica wet gel fiber; (2) The silicon oxide wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is cyclohexane), and then supercritical drying is performed to obtain silicon oxide aerogel fiber.
[0089] (3) The silica aerogel fiber prepared in step (2) is placed in a polyvinylidene fluoride (PVDF) heat shrink tube with a diameter of 1 mm and a shrinkage ratio of 6:1, and is placed in a 200°C oven for 600 s to shrink the polyvinylidene fluoride heat shrink tube. After shrinkage, the inner wall of the heat shrink tube is closely attached to the outer wall of the silica aerogel fiber to obtain an armored aerogel fiber.
[0090] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 50 μm, the thickness of the outer layer of the heat shrinkable material is 200 μm, the thickness ratio of the inner layer to the outer layer is 1:4, the porosity of the inner layer aerogel fiber material is 91%, and the specific surface area is 600 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 18MPa, and the elongation at break is about 150%.
[0091] Example 10 (1) obtaining silk fibroin wet gel fibers by wet spinning an 8.0 wt% silk fibroin original solution, specifically, extruding the 8.0 wt% silk fibroin original solution through a spinning needle with a diameter of 600 μm at an extrusion rate of 500 μL / min, and then entering an anhydrous calcium chloride / ethanol coagulation bath to obtain silk fibroin wet gel fibers; (2) Solvent replacement (the easily dry solvent used is tert-butyl alcohol) is performed on the silk fibroin wet gel fiber prepared in step (1), and then the silk fibroin aerogel fiber is obtained by freeze drying.
[0092] (3) The silk fibroin aerogel fiber of step (2) is loaded into a fluorinated ethylene propylene (FEP) heat shrinkable tube with a diameter of 1.2 mm and a shrinkage ratio of 2:1, and the tube is placed in a 120°C vacuum oven for 60 s to shrink the fluorinated ethylene propylene heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the silk fibroin aerogel fiber to obtain an armored aerogel fiber.
[0093] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 300 μm, the thickness of the outer layer of the heat shrinkable material is 200 μm, the thickness ratio of the inner layer to the outer layer is 1.5:1, the porosity of the inner layer aerogel fiber material is 96%, and the specific surface area is 223 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 21MPa, and the elongation at break is about 260%.
[0094] Embodiment 11 (1) a 20.0 wt% sodium alginate solution is wet-spinned to obtain a sodium alginate wet gel fiber, specifically, the 20.0 wt% sodium alginate solution is extruded through a needle with a diameter of 5 mm at an extrusion rate of 5000 μL / min, and then enters an anhydrous calcium chloride / water coagulation bath to obtain a sodium alginate wet gel fiber; (2) After the sodium alginate wet gel fiber in step (1) is subjected to solvent replacement (the easily dry solvent used is hexafluoroisopropanol), sodium alginate aerogel fiber is obtained by supercritical drying.
[0095] (3) The sodium alginate aerogel fiber of step (2) is loaded into an ethylene-vinyl acetate copolymer (EVA) heat shrinkable tube with a diameter of 10 mm and a shrinkage ratio of 1:1, and placed in a 50°C oven for 360 min to shrink the ethylene-vinyl acetate copolymer heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the sodium alginate aerogel fiber to obtain an armored aerogel fiber.
[0096] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 2500 μm, the thickness of the outer layer of the heat shrinkable material is 600 μm, the thickness ratio of the inner layer to the outer layer is 4.17:1, the porosity of the inner layer aerogel fiber material is 92%, and the specific surface area is 167 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 86MPa, and the elongation at break is about 900%.
[0097] Example 12 (1) A 0.1 wt% aromatic polyamide molecular solution is wet-spinned to obtain aromatic polyamide wet gel fibers, specifically, the 0.1 wt% aromatic polyamide molecular solution is extruded through a spinning needle with a diameter of 10 μm at an extrusion speed of 5 μL / min and then enters a deionized water coagulation bath to obtain aromatic polyamide wet gel fibers; (2) The aromatic polyamide wet gel fiber prepared in step (1) is subjected to solvent replacement (the easily dry solvent used is tert-butyl alcohol), and then freeze-dried to obtain aromatic polyamide aerogel fiber.
[0098] (3) The aromatic polyamide aerogel fiber prepared in step (2) is loaded into a wood grain-like heat shrinkable tube with a diameter of 0.05 mm and a shrinkage ratio of 3:1, and the tube is placed in a 600° C. oven for 1 s to shrink the wood grain-like heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the aromatic polyamide aerogel fiber to obtain armored aerogel fiber.
[0099] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 8 microns, the thickness of the outer layer of the heat shrinkable material is 30 microns, the thickness ratio of the inner layer to the outer layer is 4:15, the porosity of the inner layer aerogel fiber material is 98%, and the specific surface area is 190 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 10MPa, and the elongation at break is about 360%.
[0100] Example 13 (1) obtaining aromatic polyamide wet gel fibers by wet spinning a 5.0 wt% aromatic polyamide nanofiber dispersion, specifically, extruding the 5.0 wt% aromatic polyamide nanofiber dispersion through a needle with a diameter of 1400 μm at an extrusion speed of 2000 μL / min and then entering a deionized water coagulation bath to obtain aromatic polyamide wet gel fibers; (2) The aromatic polyamide wet gel fiber prepared in step (1) is subjected to solvent replacement (the easily dry solvent used is methanol), and then subjected to supercritical drying to obtain aromatic polyamide aerogel fiber.
[0101] (3) The aromatic polyamide aerogel fiber prepared in step (2) is loaded into a polyethylene heat shrinkable tube with a diameter of 8 mm and a shrinkage ratio of 4:1, and placed in a 120° C. oven for 30 s to shrink the polyethylene heat shrinkable tube. After shrinkage, the inner wall of the heat shrinkable tube is closely attached to the outer wall of the aromatic polyamide aerogel fiber to obtain armored aerogel fiber.
[0102] The thickness of the inner layer of the armored aerogel fiber obtained in this embodiment is 1000 μm, the thickness of the outer layer of the heat shrinkable material is 500 μm, the thickness ratio of the inner layer to the outer layer is 2:1, the porosity of the inner layer aerogel fiber material is 99%, and the specific surface area is 340 m 2 / g, the maximum tensile breaking strength of the armored aerogel fiber is about 18MPa, and the elongation at break is about 1200%.
[0103] Comparative Example 1 (1) A 3.0 wt% aromatic polyamide nanofiber dispersion was used as spinning solution A, and water was used as spinning solution B. The spinning solution A and the spinning solution B were simultaneously extruded into a water coagulation bath at an extrusion rate of 300 μL / min through a coaxial needle (inner 22G-outer 17G) to obtain a hollow aromatic polyamide wet gel fiber.
[0104] (2) The hollow aromatic polyamide wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is ethanol), and then supercritical drying is performed to obtain the hollow aromatic polyamide aerogel fiber.
[0105] (3) The hollow aromatic polyamide aerogel fiber prepared in step (2) is immersed in a 15 wt% thermoplastic elastomer (TPU) / N,N-dimethylformamide (DMF) solution and dried in an oven at 80°C to obtain an armored aerogel fiber.
[0106] The actual pictures of the aerogel fibers before and after armoring obtained in this comparative example are as follows: Figure 8 As shown, the armored aerogel fibers were severely shrunk and deformed, and a specific surface area test was performed. The armored aerogel fibers had no specific surface area and the mesoporous structure was destroyed.
[0107] Comparative Example 2 (1) A 3.0 wt% aromatic polyamide nanofiber dispersion was used as spinning solution A, and water was used as spinning solution B. The spinning solution A and the spinning solution B were simultaneously extruded into a water coagulation bath at an extrusion rate of 300 μL / min through a coaxial needle (inner 22G-outer 17G) to obtain a hollow aromatic polyamide wet gel fiber.
[0108] (2) The hollow aromatic polyamide wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is ethanol), and then supercritical drying is performed to obtain the hollow aromatic polyamide aerogel fiber.
[0109] (3) The hollow aromatic polyamide aerogel fiber prepared in step (2) was loaded into a polyethylene heat shrinkable tube with a diameter of 1.5 mm and a shrinkage ratio of 2:1, and placed in a 700° C. tubular furnace for 15 seconds to shrink the polyethylene heat shrinkable tube.
[0110] The actual pictures of the aerogel fibers before and after armoring obtained in this comparative example are as follows: Fig. 9 As shown, the armored aerogel fibers are severely shrunk, deformed and carbonized.
[0111] Comparative Example 3 (1) A 3.0 wt% aromatic polyamide nanofiber dispersion was used as spinning solution A, and water was used as spinning solution B. The spinning solution A and the spinning solution B were simultaneously extruded into a water coagulation bath at an extrusion rate of 300 μL / min through a coaxial needle (inner 22G-outer 17G) to obtain a hollow aromatic polyamide wet gel fiber.
[0112] (2) The hollow aromatic polyamide wet gel fiber of step (1) is subjected to solvent replacement (the easily dry solvent used is ethanol), and then supercritical drying is performed to obtain the hollow aromatic polyamide aerogel fiber.
[0113] (3) The hollow aromatic polyamide aerogel fiber prepared in step (2) was placed in a polyethylene heat shrinkable tube with a diameter of 1.5 mm and a shrinkage ratio of 2:1, and placed in a 40° C. oven for 15 seconds to shrink the polyethylene heat shrinkable tube.
[0114] The actual pictures of the aerogel fibers before and after armoring obtained in this comparative example are as follows: Fig.10 As shown, the inner wall of the heat shrinkable tube cannot be closely attached to the outer wall of the aromatic polyamide aerogel fiber, and armored aerogel fiber cannot be obtained.
[0115] Through Examples 1-13 and Comparative Examples 1-3, it can be found that the armored aerogel fiber obtained by the above technical solution of the present invention has the characteristics of high specific surface area, high strength, high flexibility, etc., and the preparation and armoring processes are simple and easy to carry out large-scale production.
[0116] It should be understood that the order of the various steps or the order in which a particular action is performed is not very important, as long as the teachings of the present invention remain operable. In addition, two or more steps or actions may be performed simultaneously.
[0117] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.
Claims
1. An armored aerogel fiber, It is characterized in that include: The inner layer and the outer layer are coaxially structured, the outer layer is closely fitted to the outer wall of the inner layer, the inner layer comprises an aerogel fiber material having a continuous three-dimensional multi-level pore network structure, and the outer layer comprises a dense heat-shrinkable material.
2. The armored aerogel fiber according to claim 1, Features: The heat-shrinkable material includes a heat-shrinkable plastic material, preferably including any one or a combination of two or more of polyvinyl chloride heat-shrinkable tube, polyethylene heat-shrinkable tube, polyethylene terephthalate heat-shrinkable tube, ethylene-vinyl acetate copolymer heat-shrinkable tube, glue-containing double-wall heat-shrinkable tube, imitation wood grain heat-shrinkable tube, polyolefin heat-shrinkable tube, cross-linked polyolefin heat-shrinkable tube, polytetrafluoroethylene heat-shrinkable tube, fluorinated ethylene propylene heat-shrinkable tube, perfluoroalkoxy resin heat-shrinkable tube, and polyvinylidene fluoride heat-shrinkable tube; and / or, the shrinkage ratio of the heat-shrinkable material is 1:1~6:1; and / or, the shrinkage temperature of the heat-shrinkable material is 50°C~600°C.
3. The armored aerogel fiber according to claim 1, Features: The three-dimensional multi-level pore network structure includes micropores with a pore size of less than 2 nm, mesopores with a pore size of 2 to 50 nm, and macropores with a pore size of 50 nm to 100 nm; and / or the density of the inner layer of aerogel fiber material is 0.001 to 1 g / cm 3 The porosity is 1.0-99.9%, and the specific surface area is 1-1000 m 2 / g; And / or, the material of the aerogel fiber material of the inner layer includes any one or a combination of two or more of aromatic polyamide, chitosan, sodium alginate, graphene, MXene, cellulose, silk fibroin, silicon oxide, polyimide, carbon nanotubes, boron nitride, and carbon aerogel; And / or, the aerogel fiber material of the inner layer includes any one of or a combination of medium-sized aerogel fibers and non-medium-sized aerogel fibers.
4. The armored aerogel fiber according to claim 1, Features: The armored aerogel fiber has a tensile strength of 10 to 3000 MPa and an elongation at break of 1 to 3000%; And / or, the diameter of the inner layer is 0.001-100 mm; And / or, the diameter of the outer layer is 0.002-100 mm; And / or, the thickness ratio of the inner layer of aerogel fiber material to the outer layer of heat shrinkable material is 2000:1~1:1000.
5. A method for preparing armored aerogel fiber, It is characterized in that include: The aerogel fiber is sheathed in a heat-shrinkable material, and heated to the shrinkage temperature of the heat-shrinkable material, so that the heat-shrinkable material shrinks and closely adheres to the outer wall of the aerogel fiber, thereby obtaining the armored aerogel fiber.
6. The preparation method according to claim 5, Features: The heat-shrinkable material includes a heat-shrinkable plastic material, preferably including any one or a combination of two or more of polyvinyl chloride heat-shrinkable tube, polyethylene heat-shrinkable tube, polyethylene terephthalate heat-shrinkable tube, ethylene-vinyl acetate copolymer heat-shrinkable tube, glue-containing double-wall heat-shrinkable tube, imitation wood grain heat-shrinkable tube, polyolefin heat-shrinkable tube, cross-linked polyolefin heat-shrinkable tube, polytetrafluoroethylene heat-shrinkable tube, fluorinated ethylene propylene heat-shrinkable tube, perfluoroalkoxy resin heat-shrinkable tube, and polyvinylidene fluoride heat-shrinkable tube; and / or, the shrinkage ratio of the heat-shrinkable material is 1:1~6:1; And / or, the shrinkage temperature of the heat shrinkable material is 50°C to 600°C; And / or, the diameter of the heat shrinkable material is 0.002-100 mm; And / or, the heating shrinkage time is 1s to 6h.
7. The preparation method according to claim 5, It is characterized in that include: The spinning solution is subjected to a spinning technique to obtain a wet gel fiber; The wet gel fiber is dried to obtain aerogel fiber.
8. The preparation method according to claim 7, Features: The spinning solution includes any one or a combination of two or more of an aromatic polyamide nanofiber dispersion, an aromatic polyamide molecular solution, a chitosan solution, a sodium alginate solution, a graphene oxide dispersion, a MXene dispersion, a cellulose nanofiber dispersion, a cellulose nanocrystal solution, a silk fibroin solution, a silica sol, a polyimide precursor solution, a carbon nanotube dispersion, a boron nitride precursor solution, and a carbon precursor solution; And / or, the spinning technology includes any one or a combination of two or more of gel spinning technology, wet spinning technology, dry spinning technology, dry-jet wet spinning technology, dry-freeze spinning technology, 3D printing technology, mold filamentation technology, coaxial wet spinning technology, coaxial 3D printing technology, and coaxial dry-freeze spinning technology, preferably including any one or a combination of two of wet spinning technology and coaxial wet spinning technology; Preferably, the wet spinning technology comprises: providing a spinning solution of a selected concentration, and extruding the spinning solution into a coagulation bath through a spinneret or a spinning needle to form a wet gel fiber; wherein the process conditions adopted by the wet spinning technology include: the concentration of the spinning solution is 0.1 to 20 wt%, the diameter of the spinning needle is 10 to 5000 μm, and the extrusion speed is 5 to 5000 μL / min; Preferably, the coaxial wet spinning technology comprises: providing a first spinning solution of a selected concentration, using a selected solvent as a second spinning solution, and simultaneously extruding the first spinning solution and the second spinning solution into a coagulation bath through a hollow spinneret or a coaxial needle to obtain a wet gel fiber; wherein the process conditions adopted by the coaxial wet spinning technology include: the concentration of the first spinning solution is 0.1 to 20 wt%, the extrusion speed of the first spinning solution is 5 to 5000 μL / min, and the extrusion speed of the second spinning solution is 5 to 5000 μL / min; the selected solvent includes any one of water, a metal ion aqueous solution, an acid solution, an alkaline solution, and an organic solvent, or a combination of two or more thereof; Preferably, the coagulation bath used in the wet spinning technology and the coaxial wet spinning technology includes a main component and an auxiliary component, wherein the main component includes any one of water, ethanol, acetone, acetic acid, dimethyl sulfoxide, nitrogen methyl pyrrolidone, ethyl acetate, dimethyl silicone oil, and N,N-dimethylformamide, or a combination of two or more thereof; the auxiliary component includes any one of sulfuric acid, hydrochloric acid, ascorbic acid, calcium chloride, ferric chloride, potassium hydroxide, sodium hydroxide, and ammonium hydroxide, or a combination of two or more thereof; and particularly preferably, the mass ratio of the main component to the auxiliary component is 1:0 to 1:99; And / or, the preparation method comprises: first replacing the non-drying solvent in the wet gel fiber with an easy-drying solvent, and then drying the replaced wet gel fiber, wherein the easy-drying solvent comprises any one or a combination of two or more of water, methanol, ethanol, tert-butanol, hexafluoroisopropanol, acetone, cyclohexane and n-hexane; And / or, the drying process includes any one or a combination of two or more of supercritical fluid drying, vacuum freeze drying, reduced pressure drying and normal pressure drying.
9. Armored aerogel fiber prepared by the preparation method according to any one of claims 5 to 8.
10. Application of the armored aerogel fiber according to any one of claims 1 to 4 and 9 in the fields of anti-gravity liquid transport, pipeline drag reduction, thermal management, smart fabrics, wearable devices, environmental management, sensing, sound absorption and noise reduction, thermal insulation, optics, textiles or microfluidics.
Citation Information
Patent Citations
Flexible packaging aerogel composite material and preparation method thereof
CN116376267A
Preparation method of super-stretchable aerogel fiber with oriented pore structure
CN117328156A
Cited By
Superfine high-strength meta-aramid fiber and preparation method thereof
CN119685946A