Titanium-based flame-retardant polyester fiber and preparation method thereof

By combining modified polyester resin and titanium dioxide, the flame retardancy and mechanical properties of polyester fibers are increased, and the problems of release of harmful gases in existing polyester fibers are solved, achieving the non-release of toxic gases and reducing the release of toxic gases. cost effect.

CN119061518AActive Publication Date: 2024-12-03JIANGSU XUANDA POLYMER MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411390415.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-03
Estimated Expiration
2044-10-08

AI Technical Summary

Technical Problem

The flame retardant used in existing polyester fibers releases harmful gases at high temperatures, which increases costs and affects performance. A fiber that does not release toxic gases, reduces costs and has a good flame retardant effect is urgently needed.

Method used

By preparing modified polyester resin and modified titanium dioxide, phosphate groups and alkane segments are added, and pentaerythritol phosphate in cage-like structures is combined to increase the flame retardancy and mechanical properties of the polyester fibers, and through silane coupling agent Titanium dioxide is modified to improve its dispersion and compatibility to form titanium-based flame retardant polyester fibers.

Benefits of technology

The good flame retardancy, extinction and mechanical properties of polyester fiber are achieved, while avoiding the release of toxic gases, reducing the amount of flame retardant added, improving the toughness and ultraviolet resistance of the fibers, and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005072248800000091
    Figure BDA0005072248800000091
  • Figure BDA0005072248800000101
    Figure BDA0005072248800000101
Patent Text Reader

Abstract

The invention relates to the technical field of polyester fiber preparation, in particular to a titanium-based flame-retardant polyester fiber and a preparation method thereof.The polyester fiber is prepared from, by weight, 95-110 parts of modified polyester resin, 0.5-1 part of modified titanium dioxide, 0.5-1.5 parts of flame retardant and 0.5-1 part of antioxidant. The titanium-based flame-retardant polyester fiber prepared by the invention has good mechanical properties and matting property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyester fiber preparation, and in particular to a titanium-based flame-retardant polyester fiber and a preparation method thereof. Background Art

[0002] Polyester fiber is a type of synthetic fiber, usually a polymer compound made by esterification of terephthalic acid and ethylene glycol. Polyester fiber has the advantages of good elasticity, high strength and excellent wear resistance. It is widely used in clothing, home textiles, and decorations, becoming one of the most widely used fibers in the current textile industry. However, traditional polyester fiber is flammable fiber. Many fire accidents are caused or expanded by the burning of textiles. Therefore, increasing the flame retardancy of polyester fiber is of great significance to eliminating fire hazards, delaying the spread of fire, and reducing harm to people's bodies.

[0003] Patent CN106521691B discloses a polyester fiber with flame retardant and antibacterial properties, which is made of polyester resin, polyimide, nano-bentonite, basalt fiber, 8-hydroxyquinoline copper, flame retardant, starch ether, initiator, silane coupling agent, dispersant, and surfactant. The polyester fiber prepared by this invention has excellent antibacterial and flame retardancy, but the flame retardant used in this invention contains halogen. Halogen-containing flame retardants will release harmful gases at high temperatures, which is harmful to human health.

[0004] Patent CN112831863B discloses a flame-retardant polyester fiber and its preparation process, which is composed of 70-80 parts of polyester chips, 18-30 parts of flame-retardant masterbatch and 2.0-5.0 parts of anti-dripping agent; wherein the flame-retardant masterbatch is composed of a composite flame retardant, a synergistic flame retardant, urea, nano-titanium dioxide, nano-bamboo charcoal powder, an antioxidant, calcium stearate, ethylene bis fatty acid amide, isopropyl tri(dioctyl pyrophosphate) titanate and polyester chips; under the synergistic effect of various substances, the prepared polyester fiber has a better flame retardant effect. The invention adopts a blending method to add the flame-retardant masterbatch to the polyester fiber, which usually requires the addition of more flame retardants, which increases the cost to a certain extent.

[0005] Therefore, there is an urgent need in the market for a polyester fiber that does not release toxic gases, has reduced costs and has good flame retardant effects. Summary of the invention

[0006] In order to overcome the above-mentioned deficiencies of the prior art, the present invention provides a titanium-based flame-retardant polyester fiber which does not release toxic gases, can reduce costs to a certain extent, and has good matting and mechanical properties.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] The first aspect of the present invention provides a titanium-based flame-retardant polyester fiber, which comprises the following raw materials, in parts by weight: 95-110 parts of modified polyester resin, 0.5-1 part of modified titanium dioxide, 0.5-1.5 parts of flame retardant, and 0.5-1 part of antioxidant.

[0009] In some embodiments, the method for preparing the modified polyester resin comprises the following steps:

[0010] (1) adding pentaerythritol phosphate, maleic anhydride and phosphoric acid to dichloromethane, reacting at 70-80° C. for 5-6 hours, rotary evaporating and drying to obtain a compound; adding the obtained compound, 4-vinylbenzoic acid and azobisisobutyronitrile to methanol, reacting at 70-80° C. for 0.5-1.5 hours to obtain a copolymer with a number average molecular weight of 300-400;

[0011] (2) adding terephthalic acid, ethylene glycol, a catalyst, and a heat stabilizer to a first reaction kettle, removing the air in the reaction kettle, reacting at 235-245° C. and 0.2-0.4 MPa, and when the water output reaches 85-90% of the theoretical value, adding polyethylene glycol at normal pressure, reacting at normal pressure for 50-70 minutes, and when the water output reaches 95-99% of the theoretical value, ending the reaction to obtain a reaction liquid;

[0012] (3) The reaction liquid obtained in step (2) is transported to a second reaction kettle, the temperature reaches 240-250° C., and the copolymer obtained in step (1) is added while stirring. The pressure in the kettle is reduced to -0.1 KPa to 1 KPa within 45-55 minutes, and the temperature in the kettle is controlled at 275-285° C. The reaction is carried out for 1-2 hours, and then the pressure in the kettle is increased to 40-50 Pa. The reaction time is 4-5 hours, and the material is discharged, pelletized, and dried to obtain a modified polyester resin.

[0013] Polyester fiber is flammable. In order to improve the flame retardancy of polyester fiber, it is usually necessary to add flame retardant. However, directly adding flame retardant may lead to uneven distribution and affect the flame retardant effect. The present invention modifies polyester fiber to give polyester fiber flame retardancy, which can reduce the amount of flame retardant added. The possible reason is that phosphate groups are added to the modified polyester fiber to make it flame retardant. In addition, copolymers containing alkane segments and benzene rings participate in the polycondensation reaction of polyester, which increases the free alkane segments. On the one hand, the irregularity of the polyester fiber structure is increased, and the toughness of the polyester fiber is increased. In addition, the free alkane segments increase the entanglement of phosphate and the main chain of the polyester fiber, so that the phosphate can be tightly combined with the main chain, further improving the flame retardancy. At the same time, the specific selection of pentaerythritol phosphate with a cage structure increases the interaction force with flame retardants, modified titanium dioxide, etc., further increases the compatibility with polyester fiber, so that the obtained polyester fiber has uniform texture and good mechanical properties.

[0014] In some embodiments, the mass ratio of pentaerythritol phosphate to maleic anhydride in step (1) is (1.5-1.8):1.

[0015] In some embodiments, the mass ratio of the compound to 4-vinylbenzoic acid in step (1) is (1.8-2.1):1.

[0016] The invention limits pentaerythritol phosphate to react with only one carboxyl group after hydrolysis of maleic anhydride, retains one carboxyl group to participate in the esterification reaction, and then limits the mass ratio of the compound to 4-vinylbenzoic acid to make it have a certain alkane chain segment, and at the same time, have enough carboxyl groups to participate in the esterification reaction, thereby increasing the toughness of the polyester fiber.

[0017] In some embodiments, the mass ratio of terephthalic acid, ethylene glycol and polyethylene glycol in step (2) is 1:(0.2-0.4):(0.5-0.7).

[0018] In some embodiments, the mass ratio of the reaction liquid to the copolymer in step (3) is 1:(0.1-0.2).

[0019] The present invention increases the processability of polyester fiber by limiting the mass ratio of terephthalic acid, ethylene glycol and polyethylene glycol, while not reducing the water resistance of polyester; and increases the flame retardancy of the modified polyester resin by limiting the mass ratio of the reaction liquid and the copolymer, while not reducing the original performance of the polyester resin.

[0020] In some embodiments, the method for preparing the modified titanium dioxide comprises the following steps:

[0021] 1) adding 2-hydroxy-4-(methacryloyloxy)benzophenone, 10-hydroxy-2-decenoic acid and azobisisobutyronitrile to methanol, stirring and reacting at 70-80° C. for 7-8 hours to obtain a prepolymer with a number average molecular weight of 500-600;

[0022] 2) Add titanium dioxide and a silane coupling agent into ethanol, stir at 50-60° C. for 3-4 hours, then add the prepolymer obtained in step 1), stir and react at 70-80° C. for 1-2 hours to obtain modified titanium dioxide.

[0023] Preferably, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane.

[0024] Titanium dioxide has a certain matting effect and antibacterial property. It can be added to polyester fiber as a filler to increase the strength of the polyester fiber. The particle size of titanium dioxide is small, and it is difficult to disperse unevenly in the polyester fiber, resulting in uneven quality of the polyester fiber. The present invention modifies titanium dioxide to make it have good dispersibility, and it can be evenly dispersed when blended with polyester resin. The obtained polyester fiber has good matting property. The possible reason is that the modified titanium dioxide also has a polar carboxyl group, which generates a negative charge, increases the electrostatic repulsion between titanium dioxide particles, and makes it evenly dispersed. In addition, the modified titanium dioxide has better compatibility with polyester resin, and also increases the ultraviolet resistance of polyester fiber. In addition, the addition of silane coupling agent also helps to reduce surface tension, and has a tendency to migrate to the surface when heated. When burning, organic silicon dehydrates to form layered silicon dioxide, which can increase the anti-melting droplet property of polyester fiber.

[0025] In some embodiments, in step 1), the mass ratio of 2-hydroxy-4-(methacryloyloxy)benzophenone to 10-hydroxy-2-decenoic acid is 1:(0.66-0.80).

[0026] In some embodiments, in step 2), the mass ratio of titanium dioxide, silane coupling agent and prepolymer is 1:(0.5-0.7):(0.6-0.8).

[0027] The invention limits the mass ratio of 2-hydroxy-4-(methacryloyloxy)benzophenone to 10-hydroxy-2-decenoic acid so that the obtained prepolymer contains a certain carboxyl group, thereby increasing the dispersibility of the modified titanium dioxide and having good compatibility with the polyester resin. In addition, the mass ratio of titanium dioxide, a silane coupling agent and the prepolymer is limited so that part of the hydroxyl groups on the surface of the titanium dioxide reacts with the silane coupling agent, thereby reducing the agglomeration phenomenon and still maintaining good extinction properties.

[0028] A second aspect of the present invention provides a method for preparing a titanium-based flame-retardant polyester fiber, comprising the following steps:

[0029] S1. Add modified polyester resin, modified titanium dioxide, flame retardant and antioxidant into a mixer and stir for 20-30 minutes to obtain a mixture;

[0030] S2. Add the mixed material obtained in step S1 into a twin-screw extruder for extrusion. The feeding speed of the twin-screw extruder is 550-650rpm, the extrusion temperature is 240-250°C, and then melt spinning is carried out. The supply of the spinning metering pump is controlled to be 700-800g / min, the spinning temperature is 275-285°C, and the spinning speed is 840-860m / min. Then, a drafting process is carried out, the drafting multiple is 1.5-2.5 times, and the winding speed is 650-750m / min to obtain titanium-based flame-retardant polyester fiber.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The present invention has good flame retardancy, matting and UV resistance by adding copolymers and modified titanium dioxide. No toxic gas is released during the preparation process, which can reduce costs to a certain extent and has good mechanical properties.

[0033] 2. The present invention modifies polyester fiber to impart flame retardancy to the polyester fiber, thereby reducing the amount of flame retardant added. In addition, a copolymer containing an alkane chain segment and a benzene ring participates in the polycondensation reaction of the polyester, thereby increasing the free-moving alkane chain segment. On the one hand, the irregularity of the polyester fiber structure is increased, thereby increasing the toughness of the polyester fiber. On the other hand, the free-moving alkane chain segment increases the entanglement of the phosphate ester with the main chain of the polyester fiber, thereby enabling the phosphate ester to be tightly combined with the main chain, thereby further improving the flame retardancy. At the same time, a cage-like structured pentaerythritol phosphate is specifically selected to increase the interaction force with other substances, thereby increasing the compatibility with the polyester fiber, thereby making the obtained polyester fiber uniform in texture.

[0034] 3. The present invention modifies titanium dioxide to have good dispersibility and can be evenly dispersed when blended with polyester resin. The obtained polyester fiber has good extinction property. In addition, the modified titanium dioxide has better compatibility with polyester resin and also increases the UV resistance of polyester fiber. In addition, the addition of silane coupling agent also helps to reduce surface tension and has a tendency to migrate to the surface when heated. When burning, the organic silicon dehydrates to form layered silicon dioxide, which can increase the anti-melting droplet property of polyester fiber. DETAILED DESCRIPTION

[0035] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following examples and comparative examples are only used to illustrate the present invention and are not intended to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0036] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments and comparative examples are described as follows:

[0037] The compounds and related reagents used in the following examples and comparative examples can all be purchased from the market, wherein titanium dioxide was purchased from Shanghai Maoguo Nanotechnology Co., Ltd., with a particle size of 20 nm.

[0038] Preparation Example 1

[0039] The preparation method of modified polyester resin-1 comprises the following steps:

[0040] (1) 16 g of pentaerythritol phosphate, 10 g of maleic anhydride and 0.2 g of 75 wt% phosphoric acid solution were added to 100 ml of dichloromethane, reacted at 75° C. for 5.5 h, rotary evaporated and dried to obtain a compound; 20 g of the obtained compound, 10 g of 4-vinylbenzoic acid and 1 g of azobisisobutyronitrile were added to 1000 g of anhydrous methanol, reacted at 75° C. for 1 h, and a copolymer with a number average molecular weight of 367 was obtained;

[0041] (2) 10 g of terephthalic acid, 3 g of ethylene glycol, 0.1 g of ethylene glycol antimony, and 0.1 g of triphenyl phosphate were added to a first reaction kettle, the air in the reaction kettle was removed, and the reaction was carried out at 240° C. and 0.3 MPa. When the water output reached 87% of the theoretical value, 6 g of polyethylene glycol-600 was added under normal pressure, and the reaction was carried out at normal pressure for 60 min. When the water output reached 98% of the theoretical value, the reaction was terminated to obtain a reaction liquid;

[0042] (3) 10 g of the reaction liquid obtained in step (2) was transferred to the second reaction kettle, the temperature reached 245° C., and 1.5 g of the copolymer obtained in step (1) was added while stirring. The pressure in the kettle was reduced to -0.1 KPa within 50 min, and the temperature in the kettle was controlled at 280° C. The reaction was carried out for 1.5 h, and then the pressure in the kettle was increased to 46 Pa. The reaction time was 4.5 h. The material was discharged, pelletized, and dried to obtain modified polyester resin-1.

[0043] Preparation Example 2

[0044] The preparation method of modified polyester resin-2 has the same specific steps as those of Preparation Example 1, except that the amount of pentaerythritol phosphate added in step (1) is 20 g.

[0045] Preparation Example 3

[0046] The preparation method of modified polyester resin-3 has the same specific steps as Preparation Example 1, except that the amount of compound added in step (1) is 15 g.

[0047] Preparation Example 4

[0048] The preparation method of modified polyester resin-4 has the same specific steps as Preparation Example 1, except that the amount of polyethylene glycol added in step (2) is 3 g.

[0049] Preparation Example 5

[0050] The preparation method of modified polyester resin-5 has the same specific steps as Preparation Example 1, except that the amount of copolymer added in step (3) is 3 g.

[0051] Preparation Example 6

[0052] The preparation method of polyester resin comprises the following steps:

[0053] (1) 16 g of pentaerythritol phosphate, 10 g of maleic anhydride and 75 wt% phosphoric acid solution were added to 100 ml of dichloromethane, reacted at 75° C. for 5.5 h, rotary evaporated and dried to obtain a compound; 20 g of the obtained compound, 10 g of 4-vinylbenzoic acid and 1 g of azobisisobutyronitrile were added to 1000 g of anhydrous methanol, reacted at 75° C. for 1 h, to obtain a copolymer with a number average molecular weight of 367;

[0054] (2) 10 g of terephthalic acid, 3 g of ethylene glycol, 0.1 g of ethylene glycol antimony, and 0.1 g of triphenyl phosphate were added to a first reaction kettle, the air in the reaction kettle was removed, and the reaction was carried out at 240° C. and 0.3 MPa. When the water output reached 87% of the theoretical value, 6 g of polyethylene glycol-600 was added under normal pressure, and the reaction was carried out at normal pressure for 60 min. When the water output reached 98% of the theoretical value, the reaction was terminated to obtain a reaction liquid;

[0055] (3) 10 g of the reaction liquid obtained in step (2) was transferred to the second reaction kettle, the temperature reached 245° C., the pressure in the kettle was reduced to -0.1 KPa within 50 min, the temperature in the kettle was controlled at 280° C., the reaction was carried out for 1.5 h, and then the pressure in the kettle was increased to 46 Pa. The reaction time was 4.5 h, the material was discharged, pelletized, and dried to obtain a polyester resin.

[0056] Preparation Example 7

[0057] The preparation method of modified titanium dioxide-1 comprises the following steps:

[0058] 1) Add 10 g of 2-hydroxy-4-(methacryloyloxy)benzophenone, 7.5 g of 10-hydroxy-2-decenoic acid, and 0.1 g of azobisisobutyronitrile to 100 ml of anhydrous methanol, stir and react at 75° C. for 7.5 h to obtain a prepolymer with a number average molecular weight of 587;

[0059] 2) Add 10 g of titanium dioxide and 6 g of γ-methacryloxypropyltrimethoxysilane to 300 g of anhydrous ethanol, stir at 55° C. for 3.5 h, then add 7 g of the prepolymer obtained in step 1), stir and react at 75° C. for 1.5 h to obtain modified titanium dioxide-1.

[0060] Preparation Example 8

[0061] The preparation method of modified titanium dioxide-2 has the same specific steps as Preparation Example 7, except that the amount of 10-hydroxy-2-decenoic acid added in step 1) is 9 g.

[0062] Preparation Example 9

[0063] The preparation method of modified titanium dioxide-3 has the same specific steps as Preparation Example 7, except that the amount of prepolymer added in step 2) is 10 g.

[0064] Example 1

[0065] A titanium-based flame-retardant polyester fiber comprises the following raw materials, measured in parts by weight: 100 parts of modified polyester resin-1, 0.8 parts of modified titanium dioxide-1, 1 part of tricresyl phosphate, and 0.8 parts of antioxidant 1010.

[0066] The method for preparing the titanium-based flame-retardant polyester fiber in this embodiment comprises the following steps:

[0067] S1, adding modified polyester resin-1, modified titanium dioxide-1, tricresyl phosphate, and antioxidant 1010 into a mixer, stirring for 25 minutes to obtain a mixture;

[0068] S2. Add the mixed material obtained in step S1 into a twin-screw extruder for extrusion. The feeding speed of the twin-screw extruder is 600 rpm and the extrusion temperature is 245° C. Then, melt spinning is performed, the supply of the spinning metering pump is controlled to be 750 g / min, the spinning temperature is 280° C., and the spinning speed is 850 m / min. Then, a drafting process is performed with a drafting multiple of 2 times and a winding speed of 700 m / min to obtain a titanium-based flame-retardant polyester fiber.

[0069] Example 2

[0070] A titanium-based flame-retardant polyester fiber comprises the following raw materials, measured in parts by weight: 95 parts of modified polyester resin-1, 0.5 parts of modified titanium dioxide-1, 0.5 parts of tricresyl phosphate, and 0.5 parts of antioxidant 1010.

[0071] The method for preparing the titanium-based flame-retardant polyester fiber in this embodiment comprises the following steps:

[0072] S1, adding modified polyester resin-1, modified titanium dioxide-1, tricresyl phosphate, and antioxidant 1010 into a mixer, stirring for 20 minutes to obtain a mixture;

[0073] S2. Add the mixed material obtained in step S1 into a twin-screw extruder for extrusion. The feeding speed of the twin-screw extruder is 550 rpm and the extrusion temperature is 240° C. Then, melt spinning is performed, the supply of the spinning metering pump is controlled to be 700 g / min, the spinning temperature is 275° C., and the spinning speed is 840 m / min. Then, a drafting process is performed with a drafting multiple of 1.5 times and a winding speed of 650 m / min to obtain a titanium-based flame-retardant polyester fiber.

[0074] Example 3

[0075] A titanium-based flame-retardant polyester fiber comprises the following raw materials, measured in parts by weight: 1 100 parts of modified polyester resin, 1 1 part of modified titanium dioxide, 1.5 parts of tricresyl phosphate, and 1 part of antioxidant 1010.

[0076] The method for preparing the titanium-based flame-retardant polyester fiber in this embodiment comprises the following steps:

[0077] S1, adding modified polyester resin-1, modified titanium dioxide-1, tricresyl phosphate, and antioxidant 1010 into a mixer, stirring for 30 minutes to obtain a mixture;

[0078] S2. Add the mixed material obtained in step S1 into a twin-screw extruder for extrusion. The feeding speed of the twin-screw extruder is 650 rpm and the extrusion temperature is 250° C. Then, melt spinning is performed. The supply of the spinning metering pump is controlled to be 800 g / min, the spinning temperature is 285° C., and the spinning speed is 860 m / min. Then, a drafting process is performed with a drafting multiple of 2.5 times and a winding speed of 750 m / min to obtain a titanium-based flame-retardant polyester fiber.

[0079] Example 4

[0080] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified polyester resin-1 is replaced by modified polyester resin-2.

[0081] Example 5

[0082] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified polyester resin-1 is replaced by modified polyester resin-3.

[0083] Example 6

[0084] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified polyester resin-1 is replaced by modified polyester resin-4.

[0085] Example 7

[0086] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified polyester resin-1 is replaced by modified polyester resin-5.

[0087] Example 8

[0088] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified titanium dioxide-1 is replaced by modified titanium dioxide-2.

[0089] Example 9

[0090] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of modified titanium dioxide-1 is replaced by modified titanium dioxide-3.

[0091] Comparative Example 1

[0092] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified polyester resin-1 is replaced by polyester resin.

[0093] Comparative Example 2

[0094] A titanium-based flame-retardant polyester fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified titanium dioxide-1 is replaced by titanium dioxide.

[0095] Performance Testing

[0096] 1. Mechanical properties

[0097] The mechanical properties of the titanium-based flame-retardant polyester fibers prepared in the above embodiments and comparative examples were tested on a multifilament strength tester, with a pre-tension of 3 cN, a stretching speed of 200 mm / min, and a clamping distance of 200 mm.

[0098] 2. Flame retardancy

[0099] Using a high temperature oxygen index tester, the polyester fiber obtained in each embodiment and comparative example was wound on a yarn length measuring instrument for 40 m of fiber, twisted with a twist number of 130±20, folded in the middle into a strand, and the ends were fixed. The limiting oxygen index was tested with reference to the "Test method for flame retardancy of polyester fibers - oxygen index method FZT 50017-2001".

[0100] 3. Matting

[0101] Using barium sulfate as a reference sample, an integrating sphere accessory was used to collect diffuse reflectance signals of visible light of the polyester fibers obtained in various embodiments and comparative examples. The greater the diffuse reflectance of visible light, the better the extinction property.

[0102] The test results are shown in Table 1.

[0103] Table 1

[0104]

[0105]

[0106] By comparing the experimental data of Examples 1-3 in Table 1, it can be seen that the polyester fiber has good mechanical properties, flame retardancy and extinction properties; by comparing Example 4 with Example 1, it can be seen that the change in the ratio of pentaerythritol phosphate to maleic anhydride in the modified polyester resin-2 may reduce the active groups of the copolymer, affect the formation of the polyester resin, and cause the mechanical properties of the polyester fiber to decrease; by comparing Example 5 with Example 1, it can be seen that the change in the ratio of the compound to 4-vinylbenzoic acid in the modified polyester resin-3 may cause the mechanical properties and flame retardancy of the polyester fiber to decrease due to the reduction in the number of phosphate esters; by comparing Example 6 with Example 1, it can be seen that the change in the ratio of terephthalic acid, ethylene glycol and polyethylene glycol in the modified polyester resin-4 may cause the processability of the polyester fiber to decrease, resulting in a decrease in all properties; by comparing Example 7 with Example 1, it can be seen that the modified polyester The change in the ratio of the reaction liquid to the copolymer in Resin-5 may result in a decrease in the mechanical properties of the polyester fiber due to the excessive irregularity of the polyester resin; from Example 8 compared with Example 1, it can be seen that the change in the ratio of 2-hydroxy-4-(methacryloyloxy)benzophenone to 10-hydroxy-2-decenoic acid in the modified titanium dioxide-2 may lead to a decrease in the compatibility of the modified titanium dioxide with the polyester resin, and the mechanical properties and extinction of the polyester resin are both reduced; from Example 9 compared with Example 1, it can be seen that the change in the ratio of titanium dioxide, silane coupling agent and prepolymer in the modified titanium dioxide-3 leads to a decrease in the extinction of the polyester fiber; from Comparative Example 1 compared with Example 1, it can be seen that the use of unmodified polyester resin has a decrease in mechanical properties and flame retardancy; from Comparative Example 2 compared with Example 1, it can be seen that the use of unmodified titanium dioxide has a decrease in the mechanical properties of the polyester fiber.

[0107] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A titanium-based flame-retardant polyester fiber, characterized in that: The invention comprises the following raw materials in parts by weight: 95-110 parts of modified polyester resin, 0.5-1 part of modified titanium dioxide, 0.5-1.5 parts of flame retardant and 0.5-1 part of antioxidant.

2. The titanium-based flame-retardant polyester fiber according to claim 1, characterized in that: The preparation method of the modified polyester resin comprises the following steps: (1) adding pentaerythritol phosphate, maleic anhydride and phosphoric acid to dichloromethane, reacting at 70-80° C. for 5-6 hours, rotary evaporating and drying to obtain a compound; adding the obtained compound, 4-vinylbenzoic acid and azobisisobutyronitrile to methanol, reacting at 70-80° C. for 0.5-1.5 hours to obtain a copolymer with a number average molecular weight of 300-400; (2) adding terephthalic acid, ethylene glycol, a catalyst, and a heat stabilizer to a first reaction kettle, removing the air in the reaction kettle, reacting at 235-245° C. and 0.2-0.4 MPa, and when the water output reaches 85-90% of the theoretical value, adding polyethylene glycol at normal pressure, reacting at normal pressure for 50-70 minutes, and when the water output reaches 95-99% of the theoretical value, ending the reaction to obtain a reaction liquid; (3) The reaction liquid obtained in step (2) is transported to a second reaction kettle, the temperature reaches 240-250° C., and the copolymer obtained in step (1) is added while stirring. The pressure in the kettle is reduced to -0.1 KPa to 1 KPa within 45-55 minutes, and the temperature in the kettle is controlled at 275-285° C. The reaction is carried out for 1-2 hours, and then the pressure in the kettle is increased to 40-50 Pa. The reaction time is 4-5 hours, and the material is discharged, pelletized, and dried to obtain a modified polyester resin.

3. The titanium-based flame-retardant polyester fiber according to claim 2, characterized in that: In the step (1), the mass ratio of pentaerythritol phosphate to maleic anhydride is (1.5-1.8):

1.

4. The titanium-based flame-retardant polyester fiber according to claim 2, characterized in that: The mass ratio of the compound to 4-vinylbenzoic acid in the step (1) is (1.8-2.1):

1.

5. The titanium-based flame-retardant polyester fiber according to claim 2, characterized in that: In the step (2), the mass ratio of terephthalic acid, ethylene glycol and polyethylene glycol is 1:(0.2-0.4):(0.5-0.7).

6. The titanium-based flame-retardant polyester fiber according to claim 2, characterized in that: In the step (3), the mass ratio of the reaction liquid to the copolymer is 1:(0.1-0.2).

7. The titanium-based flame-retardant polyester fiber according to claim 1, characterized in that: The preparation method of the modified titanium dioxide comprises the following steps: 1) adding 2-hydroxy-4-(methacryloyloxy)benzophenone, 10-hydroxy-2-decenoic acid and azobisisobutyronitrile to methanol, stirring and reacting at 70-80° C. for 7-8 hours to obtain a prepolymer with a number average molecular weight of 500-600; 2) Add titanium dioxide and a silane coupling agent into ethanol, stir at 50-60° C. for 3-4 hours, then add the prepolymer obtained in step 1), stir and react at 70-80° C. for 1-2 hours to obtain modified titanium dioxide.

8. The titanium-based flame-retardant polyester fiber according to claim 7, characterized in that: In the step 1), the mass ratio of 2-hydroxy-4-(methacryloyloxy)benzophenone to 10-hydroxy-2-decenoic acid is 1:(0.66-0.80).

9. The titanium-based flame-retardant polyester fiber according to claim 7, characterized in that: In the step 2), the mass ratio of titanium dioxide, silane coupling agent and prepolymer is 1:(0.5-0.7):(0.6-0.8).

10. A method for preparing the titanium-based flame-retardant polyester fiber according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Add modified polyester resin, modified titanium dioxide, flame retardant and antioxidant into a mixer and stir for 20-30 minutes to obtain a mixture; S2. Add the mixed material obtained in step S1 into a twin-screw extruder for extrusion. The feeding speed of the twin-screw extruder is 550-650rpm, the extrusion temperature is 240-250°C, and then melt spinning is carried out. The supply of the spinning metering pump is controlled to be 700-800g / min, the spinning temperature is 275-285°C, and the spinning speed is 840-860m / min. Then, a drafting process is carried out, the drafting multiple is 1.5-2.5 times, and the winding speed is 650-750m / min to obtain titanium-based flame-retardant polyester fiber.

Citation Information

Patent Citations

  • Polyester fibers with flame-retardant and antibacterial properties and their applications

    CN106521691B

  • A flame-retardant polyester fiber and its preparation process

    CN112831863B

  • Uvioresistant poly (1, 2-propylene glycol terephthalate) fibre

    CN101701367A

  • Method for preparing titanium-based matte polyester fiber through direct melt spinning and product

    CN111286805A

  • Fire-retarded material of polypentaerythritol kind phosphate ester melamine salt expended type and its preparation process