Wear-resistant and corrosion-resistant satin cloth and preparation process thereof
By using the combination of polyester fiber, spandex, nylon fiber and other materials in the Sedding cloth, adding functional components such as water-based polyurethane and nitrile rubber, and using specific processes, the lack of wear and corrosion resistance of Sedding cloth is solved. The problem of this paper has achieved a significant improvement in the wear resistance and corrosion resistance of Sertin.
Patent Information
- Application Number
- CN202411151415.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to prepare a wear-resistant and corrosion-resistant Sedding cloth based on keeping the color of the Sedding cloth bright, smooth feel, elegant quality, softness and good tear resistance.
Polyester fiber, spandex, and nylon fiber are used as the substrate, and water-based polyurethane, nitrile rubber, color masterbing, ultraviolet absorber, antioxidant and emulsifier are prepared through kneading, combing, stretching, torsion and twisting processes. Wear-resistant and corrosion-resistant Salton fabric.
It significantly improves the wear resistance and corrosion resistance of Sedin cloth, making it excellent in environments in contact with oils and chemicals, enhances elasticity and resilience, and is suitable for a wider range of applications.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of satin cloth, in particular to a wear-resistant and corrosion-resistant satin cloth and a preparation process thereof. Background Art
[0002] Satin is a kind of lustrous spun fabric made of polyester or rayon. Its main component is polyester, and other functional components are added to the polyester. The surface of the prepared fabric is shiny, so it is called satin. With the continuous progress and innovation of textile technology, the production process and technical level of satin are constantly improving. The application of new technologies and new materials has significantly improved the performance and quality of satin, and also injected new vitality into the development of the satin industry.
[0003] However, preparing a wear-resistant and corrosion-resistant satin fabric while maintaining the bright color, smooth feel, elegant quality, softness and good tear resistance of the satin fabric itself has become one of the technical difficulties in this field. Summary of the invention
[0004] The invention aims at the problems existing in the prior art and discloses a wear-resistant and corrosion-resistant satin fabric and a preparation process thereof. The fabric of the invention adopts polyester fiber, spandex and nylon fiber as the base of the fabric, which can maintain the advantages of the fabric itself and increase its wear resistance. The addition of other functional components prepares the wear-resistant and corrosion-resistant satin fabric with bright color, smooth hand feeling, elegant quality, softness, good tear resistance and good wear resistance.
[0005] The present invention is achieved in that:
[0006] A wear-resistant and corrosion-resistant satin fabric, characterized in that, in parts by mass, the satin fabric is prepared from the following components:
[0007] Polyester fiber: 60-80 parts;
[0008] Spandex: 12-16 parts;
[0009] Nylon fiber: 3-7 parts;
[0010] Waterborne polyurethane: 5-8 parts;
[0011] Nitrile rubber: 5-8 parts;
[0012] Masterbatch: 3-6 parts;
[0013] UV absorber: 1 to 3 parts;
[0014] Antioxidant: 1-3 parts;
[0015] Emulsifier: 10-15 parts.
[0016] Furthermore, the mass ratio between the polyester fiber and spandex is 5:1.
[0017] Furthermore, the mass ratio between the waterborne polyurethane and the nitrile rubber is 1:1.
[0018] Furthermore, the ultraviolet absorber is one of salicylate, benzotriazole and benzophenone.
[0019] Furthermore, the antioxidant is a phenolic antioxidant.
[0020] Further, the satin fabric is prepared from the following components in parts by mass:
[0021] Polyester fiber: 70 parts;
[0022] Spandex: 14 parts;
[0023] Nylon fiber: 6 parts;
[0024] Waterborne polyurethane: 7 parts;
[0025] Nitrile rubber: 7 parts;
[0026] Masterbatch: 4 parts;
[0027] UV absorber: 2 parts;
[0028] Antioxidants: 2 parts;
[0029] Emulsifier: 13 parts.
[0030] A preparation process of wear-resistant and corrosion-resistant satin fabric, characterized in that the process is specifically as follows:
[0031] Step 1, mixing: weigh 60-80 parts of polyester fiber, 12-16 parts of spandex, 3-7 parts of nylon fiber, 5-8 parts of waterborne polyurethane, and 5-8 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20°C, time: 30-40 minutes, and mix until uniform;
[0032] Step 2: Add 3-6 parts of masterbatch, 1-3 parts of ultraviolet absorber, 1-3 parts of antioxidant, and 10-15 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0033] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0034] The beneficial effects of the present invention compared with the prior art are:
[0035] In the present invention, the wear resistance is enhanced by combining polyester fiber, spandex and nylon fiber:
[0036] The combination of polyester fiber, nitrile rubber and nylon fiber makes the prepared satin fabric extremely wear-resistant, especially in environments with oil and chemicals. Its wear resistance is better than many other composite fabrics and can significantly improve the wear resistance of satin fabric.
[0037] In the present invention, the corrosion resistance is improved by combining polyester fiber, spandex and nylon fiber:
[0038] Waterborne polyurethane has good chemical stability and can resist corrosion from a variety of chemical substances, including some common solvents and acidic and alkaline substances. The combination of waterborne polyurethane and nitrile rubber makes the prepared satin fabric extremely oil-resistant and can resist corrosion from a variety of oils and solvents, which helps to improve the corrosion resistance of satin fabric in complex environments.
[0039] In the present invention, the physical properties of satin fabric are improved by combining spandex in various components:
[0040] The addition of spandex can significantly improve the elasticity and recovery of satin, making the fabric softer, more comfortable and fit to the body. The combination of polyester fiber and nylon fiber further enhances the strength and durability of satin. The combination of multiple fibers and materials makes satin have a wider range of applications. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail by enumerating examples below. It should be noted that the specific implementation described here is only used to explain the present invention and is not used to limit the present invention.
[0042] Example 1
[0043] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0044] Step 1, mixing: weigh 70 parts of polyester fiber, 14 parts of spandex, 6 parts of nylon fiber, 7 parts of water-based polyurethane, and 7 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20°C, time: 30-40 minutes, and mix until uniform;
[0045] Step 2: Add 4 parts of masterbatch, 2 parts of ultraviolet absorber, 2 parts of antioxidant and 13 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0046] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0047] Example 2
[0048] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0049] Step 1, mixing: weigh 60 parts of polyester fiber, 12 parts of spandex, 3 parts of nylon fiber, 5 parts of water-based polyurethane, and 5 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20°C, time: 30-40 minutes, and mix until uniform;
[0050] Step 2: Add 3 parts of masterbatch, 1 part of ultraviolet absorber, 1 part of antioxidant and 10 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0051] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0052] Example 3
[0053] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0054] Step 1, mixing: weigh 80 parts of polyester fiber, 16 parts of spandex, 7 parts of nylon fiber, 8 parts of water-based polyurethane, and 8 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20℃, time: 30-40 minutes, and mix until uniform;
[0055] Step 2: Add 6 parts of masterbatch, 3 parts of ultraviolet absorber, 3 parts of antioxidant and 15 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0056] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0057] Example 4
[0058] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0059] Step 1, mixing: weigh 65 parts of polyester fiber, 13 parts of spandex, 4 parts of nylon fiber, 6 parts of water-based polyurethane, and 6 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20℃, time: 30-40 minutes, and mix until uniform;
[0060] Step 2: Add 4 parts of masterbatch, 2 parts of ultraviolet absorber, 2 parts of antioxidant and 12 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0061] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0062] Example 5
[0063] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0064] Step 1, mixing: weigh 75 parts of polyester fiber, 15 parts of spandex, 6 parts of nylon fiber, 7 parts of water-based polyurethane, and 7 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20℃, time: 30-40 minutes, and mix until uniform;
[0065] Step 2: Add 5 parts of masterbatch, 3 parts of ultraviolet absorber, 2 parts of antioxidant and 11 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0066] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0067] Example 6
[0068] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0069] Step 1, mixing: weigh 65 parts of polyester fiber, 13 parts of spandex, 6 parts of nylon fiber, 8 parts of water-based polyurethane, and 8 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20℃, time: 30-40 minutes, and mix until uniform;
[0070] Step 2: Add 4 parts of masterbatch, 1 part of ultraviolet absorber, 2 parts of antioxidant and 13 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0071] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0072] Example 7
[0073] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0074] Step 1, mixing: weigh 70 parts of polyester fiber, 14 parts of spandex, 7 parts of nylon fiber, 7 parts of water-based polyurethane, and 7 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20℃, time: 30-40 minutes, and mix until uniform;
[0075] Step 2: Add 5 parts of masterbatch, 3 parts of ultraviolet absorber, 2 parts of antioxidant and 14 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0076] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0077] Example 8
[0078] A preparation process of a wear-resistant and corrosion-resistant satin fabric in this embodiment is specifically as follows:
[0079] Step 1, mixing: weigh 60 parts of polyester fiber, 12 parts of spandex, 6 parts of nylon fiber, 7 parts of water-based polyurethane, and 7 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20℃, time: 30-40 minutes, and mix until uniform;
[0080] Step 2: Add 6 parts of masterbatch, 3 parts of ultraviolet absorber, 2 parts of antioxidant and 11 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric;
[0081] Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.
[0082] The satin fabric prepared in the above embodiment was subjected to performance testing, and the results are shown in Table 1 below:
[0083] Table 1
[0084] Tensile strength, MPa Elongation at break, % Tear strength, KN / m Example 1 119 365 48 Example 2 110 358 46 Example 3 113 360 45 Example 4 113 357 43 Example 5 115 347 46 Example 6 116 348 45 Example 7 112 354 43 Example 8 114 352 46
[0085] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.
Claims
1. A wear-resistant and corrosion-resistant satin fabric, characterized in that: The satin fabric is prepared from the following components in parts by mass: Polyester fiber: 60-80 parts; Spandex: 12-16 parts; Nylon fiber: 3-7 parts; Waterborne polyurethane: 5-8 parts; Nitrile rubber: 5-8 parts; Masterbatch: 3-6 parts; UV absorber: 1 to 3 parts; Antioxidant: 1-3 parts; Emulsifier: 10-15 parts.
2. The wear-resistant and corrosion-resistant satin fabric according to claim 1, characterized in that: The mass ratio of the polyester fiber to the spandex is 5:
1.
3. The wear-resistant and corrosion-resistant satin fabric according to claim 1, characterized in that: The mass ratio of the waterborne polyurethane to the nitrile rubber is 1:
1.
4. The wear-resistant and corrosion-resistant satin fabric according to claim 1, characterized in that: The ultraviolet absorber is one of salicylate, benzotriazole and benzophenone.
5. The wear-resistant and corrosion-resistant satin fabric according to claim 1, characterized in that: The antioxidant is a phenolic antioxidant.
6. The wear-resistant and corrosion-resistant satin fabric according to claim 1, characterized in that: The satin fabric is prepared from the following components in parts by mass: Polyester fiber: 70 parts; Spandex: 14 parts; Nylon fiber: 6 parts; Waterborne polyurethane: 7 parts; Nitrile rubber: 7 parts; Masterbatch: 4 parts; UV absorber: 2 parts; Antioxidants: 2 parts; Emulsifier: 13 parts.
7. A process for preparing a wear-resistant and corrosion-resistant satin fabric according to any one of claims 1 to 6, characterized in that: The process is specifically as follows: Step 1, mixing: weigh 60-80 parts of polyester fiber, 12-16 parts of spandex, 3-7 parts of nylon fiber, 5-8 parts of waterborne polyurethane, and 5-8 parts of nitrile rubber according to mass parts, and mix them. The mixing parameters are: temperature 120±20°C, time: 30-40 minutes, and mix until uniform; Step 2: Add 3-6 parts of masterbatch, 1-3 parts of ultraviolet absorber, 1-3 parts of antioxidant, and 10-15 parts of emulsifier to the uniform mixture of step 1 and continue to mix evenly to prepare wear-resistant and corrosion-resistant satin fabric; Step 3: The wear-resistant and corrosion-resistant satin fabric in step 2 is processed by combing, stretching, twisting and twisting to form the desired wear-resistant and corrosion-resistant satin fabric.