Wear-resistant jean fabric and preparation method thereof

By using blended fibers of spandex fibers and modified cotton fibers in denim fabrics for twill weaving, the problem of insufficient wear resistance of light and breathable denim fabrics is solved, and the wear resistance of the fabric is improved and service life is extended, which is suitable for modern clothing. need.

CN119061558APending Publication Date: 2024-12-03GUANGDONG VOCATIONAL & TECHNICAL COLLEGE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411484677.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When existing denim fabrics pursue lightness, breathability and comfort, they lack wear resistance, resulting in a short service life and are difficult to meet the needs of modern consumers for durability and aesthetics.

Method used

Spandex fiber is used as the inner core, and the blended mixed fiber of modified cotton fiber and polyester fiber is combined for twill weaving. Through twisting, pre-shrinking and low-temperature dyeing, a wear-resistant denim fabric is prepared to ensure that the fabric is maintained. Soft, breathable and lightweight while having good wear resistance.

Benefits of technology

It significantly improves the wear resistance and service life of the fabric, meets the requirements of modern consumers for comfort, durability and aesthetics, and has good production technology and environmentally friendly characteristics, and is suitable for various clothing products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061558A_ABST
    Figure CN119061558A_ABST
Patent Text Reader

Abstract

The invention provides a wear-resistant jean fabric and a preparation method thereof, and relates to the technical field of jean fabrics. The wear-resistant jean fabric is prepared by twill weaving, preshrinking, dyeing and shaping of core-spun yarn with spandex fiber as an inner layer core and modified cotton fiber and polyester fiber blended mixed fiber as a coating layer. The spandex fibers are used as the inner layer core, and the blended mixed fibers of the modified cotton fibers and the polyester fibers are combined, so that the wear resistance of the fabric is improved, and the service life is prolonged. According to the jean fabric, the low-ampere design is adopted, the softness, breathability and lightness and thinness of the fabric are kept, the fabric is more suitable for daily wearing, and the wearing comfort is improved. The wear-resistant jean fabric meets the requirements of modern consumers for comfort, durability and attractiveness, has good production process and environmental protection characteristics, can have competitiveness in the market, and is suitable for various clothing products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of denim fabrics, and in particular to a wear-resistant denim fabric and a preparation method thereof. Background Art

[0002] Denim is a durable textile material commonly used to make jeans, jackets and other clothing. Denim has the advantages of durability and easy care, but it is relatively hard and has poor breathability.

[0003] Lightweight denim fabric is made by reducing the thickness of traditional denim. It provides better comfort and breathability while maintaining the classic look of denim. However, lightweight denim fabric will significantly reduce the durability of denim fabric. Its wear resistance is not as good as traditional heavy denim. Long-term wear or frequent washing will cause wear or holes more quickly.

[0004] It can be seen that the problem existing in the prior art is that it is difficult for denim fabric to have good wear resistance while being light, thin, comfortable and breathable. Therefore, it is particularly important to develop a light, thin, breathable and wear-resistant denim fabric. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a wear-resistant denim fabric and a preparation method thereof. The fabric described in the present invention has good wear resistance, and the present invention provides a low-security denim fabric, that is, it can ensure that the fabric has good wear resistance while ensuring that the fabric is soft, breathable, and thin.

[0006] The invention provides a wear-resistant denim fabric, which is prepared by core-spun yarn with spandex fiber as an inner core and modified cotton fiber and polyester fiber blended mixed fiber as a covering layer through twill weaving, pre-shrinking, dyeing and shaping.

[0007] Preferably, the wear-resistant denim fabric comprises the following raw materials in percentage by mass: 50%-70% modified cotton fiber, 20%-30% polyester fiber, and 5%-20% spandex fiber.

[0008] Preferably, the warp and weft density of the wear-resistant denim fabric is 6-10 oz.

[0009] Preferably, the modified cotton fiber is prepared by modifying cotton fiber with chitosan and a silane coupling agent.

[0010] The present invention provides a process for preparing a wear-resistant denim fabric, comprising the following steps:

[0011] The modified cotton fiber and the polyester fiber are spun and twisted to form a coating layer mixed fiber; the coating layer mixed fiber is coated on the outside of the spandex fiber to obtain a wear-resistant core-spun yarn, and the wear-resistant core-spun yarn is twill-woven, pre-shrunk, dyed and shaped to obtain a wear-resistant denim fabric.

[0012] Preferably, the twisting step comprises: twisting the yarn to a degree of 5-8 T / cm, with the twist direction being Z twist.

[0013] Preferably, in the twill weave, the warp yarn density is 27-32 yarns / cm, the weft yarn density is 13-20 yarns / cm, and the weave is performed according to 3 / 1 twill, 2 / 1 twill or 2 / 3 reinforced twill variable twill structure.

[0014] Preferably, the pre-shrinkage temperature is 170°C-200°C.

[0015] Preferably, the dyeing is low-temperature dyeing, and the dye is a disperse dye.

[0016] Compared with the prior art, the present invention improves the wear resistance of the fabric and prolongs its service life by using spandex fiber as the inner core and combining the blended mixed fiber of modified cotton fiber and polyester fiber. The denim fabric of the present invention adopts a low safety number design to maintain the softness, breathability and lightness of the fabric, making the fabric more suitable for daily wear and improving the comfort of wearing. The wear-resistant denim fabric of the present invention not only meets the requirements of modern consumers for comfort, durability and aesthetics, but also has good production technology and environmental protection characteristics, can be competitive in the market, and is suitable for various clothing products. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The present invention will be further described below in conjunction with the accompanying drawings.

[0018] Figure 1 This is a schematic diagram of the core-spun yarn structure of the present invention;

[0019] Figure 2 It is a schematic cross-sectional view of the core-spun yarn of the present invention;

[0020] In the figure, 1- cladding layer; 2- inner core. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Unless otherwise defined, all professional terms used hereinafter have the same meaning as those skilled in the art generally understand. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0022] An embodiment of the present invention provides a wear-resistant denim fabric, which is prepared by a twill weaving process using core-spun yarn with spandex fiber as an inner core and modified cotton fiber and polyester fiber blended mixed fiber as a covering layer.

[0023] The wear-resistant denim fabric provided by the present invention is a low-security denim fabric, which can ensure good wear resistance while ensuring the fabric is soft, breathable, light and thin.

[0024] Core-Spun Yarn is a mixed fiber composed of different fiber materials. Its main feature is that one fiber is used as the core fiber and then covered with other fibers as the outer fiber. This structure can combine the advantages of different fibers, so that the yarn and the fabric made of it have specific functionality and comfort.

[0025] Cotton fiber is a natural fiber that is widely used in textile production. It has the characteristics of being soft and comfortable, moisture-absorbent and breathable, heat-resistant, alkali-resistant, and environmentally friendly and sustainable.

[0026] Polyester fiber, also known as polyester, is a synthetic fiber that is widely used in the textile industry due to its superior properties. Polyester fiber is very strong, durable, and wrinkle-resistant. Compared with cotton fiber, it has stronger wear resistance, quick drying, and excellent dyeing properties.

[0027] Spandex is a polyurethane-based synthetic fiber, which is a block copolymer. The soft segment provides the elasticity of the fiber, and the hard segment provides strength and stability. This molecular structure allows the soft segment of spandex to stretch when stretched, while the hard segment maintains the overall strength of the fiber. After release, the soft segment returns to its original state, thus showing excellent elasticity.

[0028] The core-spun yarn in the embodiment of the present invention is composed of a core yarn and a covering layer, wherein the core yarn is spandex. Using spandex as the core yarn can provide good elasticity and strength for the core-spun yarn. The covering layer is a blended fiber of modified cotton fiber and polyester fiber. Using the blended fiber as the covering layer can improve the wear resistance of the core-spun yarn and give the yarn a good appearance and feel.

[0029] In some specific embodiments of the present invention, the wear-resistant denim fabric comprises the following raw materials in percentage by mass: 50%-70% modified cotton fiber, 20%-30% polyester fiber, and 5%-20% spandex fiber.

[0030] In a specific embodiment, the wear-resistant denim fabric comprises the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber. This fabric can provide good comfort and breathability after twill weaving, while ensuring the elasticity of the fabric.

[0031] In a specific embodiment, the wear-resistant denim fabric comprises the following raw materials in mass percentage: 60% modified cotton fiber, 30% polyester fiber, and 10% spandex fiber. This fabric increases the proportion of polyester fiber, enhances the wear resistance and elasticity of the fabric, and is suitable for tight-fitting design.

[0032] In a specific embodiment, the wear-resistant denim fabric comprises the following raw materials in percentage by mass: 50% modified cotton fiber, 30% polyester fiber, and 20% spandex fiber. This fabric increases the proportion of spandex, making the fabric have better elasticity and sports performance while maintaining a certain degree of comfort.

[0033] In some preferred embodiments, the method for preparing the modified cotton fiber comprises the following steps:

[0034] Chitosan and silane coupling agent are added to water to prepare a treatment solution, wherein the chitosan concentration is preferably 5-10 g / L, and the silane coupling agent concentration is preferably 4-8 g / L, and the cotton fiber is immersed in the treatment solution, and the immersion time is preferably 2-3 hours, and then dried and baked, and the baking temperature is preferably 120°C-130°C, and the baking time is preferably 5-10 minutes, to obtain modified cotton fiber. The present invention does not limit the drying method, drying temperature and drying time, and the specific drying process can be determined according to actual needs, as long as the fabric drying effect can be achieved.

[0035] In some preferred embodiments, the treatment solution further comprises 5-10 g / L of citric acid. When the treatment solution comprises citric acid, the immersion time is preferably 0.5-1.5 h.

[0036] In the embodiment of the present invention, modified cotton fiber and polyester fiber are blended in a certain proportion to form mixed fiber, so that the mixed fiber combines the softness, breathability and moisture absorption of modified cotton fiber with the high strength, wear resistance and wrinkle resistance of polyester fiber, thereby obtaining a lighter and thinner denim fabric.

[0037] The warp and weft density refers to the weight of the fabric and is an important indicator for measuring the thickness and quality of denim fabric. Generally speaking, the larger the value, the thicker the denim fabric. According to weight, denim fabrics are divided into light (6-10oz), medium weight (10-14.5oz), and heavy weight denim (14.5oz and above).

[0038] In some specific embodiments, the warp and weft density of the wear-resistant denim fabric is 6-10 oz. It can be seen that the specific embodiment of the present invention provides a thin and wear-resistant denim fabric.

[0039] The present invention provides a preparation process of wear-resistant denim fabric, comprising the following steps:

[0040] The modified cotton fiber and the polyester fiber are spun and twisted to form a coating layer mixed fiber; the coating layer mixed fiber is coated on the outside of the spandex fiber to obtain a wear-resistant core-spun yarn, and the wear-resistant core-spun yarn is twill-woven, pre-shrunk, dyed and shaped to obtain a wear-resistant denim fabric.

[0041] In some specific embodiments, the steps of preparing the coating layer mixed fiber include:

[0042] Modified cotton fiber and polyester fiber are taken out in proportion, mixed and sent to a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, which are then twisted to form a coating layer mixed fiber.

[0043] In some preferred embodiments, before preparing the mixed fiber, the raw materials are pretreated as follows:

[0044] Use clean water to soak cotton fiber and polyester fiber, spin dry and then dry, then loosen the fiber, break the fiber into fiber bundles and put them into the carding machine for combing, comb out impurities and short fibers to ensure the uniformity of the fiber.

[0045] In some preferred embodiments, the pretreatment of the mixed fiber raw material further includes a softening treatment and / or an antistatic treatment, including the following steps:

[0046] The modified cotton fiber and polyester fiber washed with clean water are soaked in a softener and / or an antistatic treatment agent, or the modified cotton fiber and polyester fiber washed with clean water are rinsed with a softener and / or an antistatic treatment agent.

[0047] In some preferred embodiments, the mixed fiber is pretreated as follows before preparing the core-spun yarn: the mixed fiber is cleaned, soaked in a detergent at room temperature, and gently scrubbed after soaking to remove grease and stains on the yarn surface.

[0048] Twist Level refers to the number of twists per meter of yarn, and twisting is the winding of fibers by rotation. Yarns with high twist are stronger, more wear-resistant and more durable, but have reduced elasticity.

[0049] Z twist means the helical direction of the fiber is the same as the middle part of the letter "Z".

[0050] In some specific embodiments, the twisting step includes: twisting the yarn to 5-8 T / cm, and the twist direction is Z twist. Twisting the warp and weft yarns can enhance the strength, wear resistance and elasticity of the yarn, making the fabric more durable.

[0051] Twill weaving is a common textile process, mainly used to produce fabrics with twill texture. It is different from plain weaving. It forms a unique diagonal pattern on the surface of the fabric through the interlaced warp and weft yarns, which enhances the structural strength and layered appearance of the fabric.

[0052] The embodiment of the present invention adopts a twill weaving method to prepare the wear-resistant denim fabric, and the surface of the obtained wear-resistant denim fabric presents oblique lines. The wear resistance of the denim fabric is ensured by the twill weaving method.

[0053] In some specific embodiments, the warp yarn density in the twill weaving is 27-32 yarns / cm, the weft yarn density is 13-20 yarns / cm, and the weaving is performed according to 3 / 1 twill, 2 / 1 twill or 2 / 3 reinforced twill variable twill structure.

[0054] In 3 / 1 twill, after the warp covers 3 wefts, the weft covers 1 warp, forming a more obvious twill effect. The warp dominates the surface of the fabric woven in this way, the twill angle is large, about 45°, and the warp strength of the fabric is high. In 2 / 1 twill, after the warp covers 2 wefts, the weft covers 1 warp. Compared with 3 / 1 twill, 2 / 1 twill has a smaller twill angle, a more balanced coverage ratio of warp and weft, a softer feel, more weft, a smoother surface and a softer feel. In 2 / 3 reinforced twill, after the weft covers 3 warps, the warp covers 2 wefts. This weaving method emphasizes the weft, and the weft dominates the surface of the fabric. The fabric is softer in the warp direction and tighter in the weft direction. Due to the dominance of the weft, the fabric is more suitable for showing soft and comfortable characteristics, but still maintains a high weft strength. At the same time, the weft density of the fabric is large, which helps to maintain the shape of the fabric. Therefore, in some preferred embodiments, the weaving is performed according to a 3 / 1 twill or 2 / 3 reinforced twill variation twill structure.

[0055] Modified cotton, polyester and spandex have different shrinkage rates, especially modified cotton, which is easy to shrink under washing and hot and humid conditions, while polyester has a lower shrinkage rate and spandex is sensitive to temperature. This difference in shrinkage rate can cause uneven shrinkage of the fabric after use or washing. The warp and weft of twill fabrics are arranged in a diagonal structure, and the shrinkage behavior of different fibers is inconsistent, which can cause the fabric to deform, warp, twist or irregular wrinkles, especially in places where the warp and weft density are greatly different.

[0056] Spandex fibers provide higher elasticity, while modified cotton fibers and polyester fibers have relatively low elasticity. In twill weaving, the oblique fiber structure increases the area affected by inconsistent elasticity, especially in areas where the fabric is often stretched. Spandex is mainly used to provide elasticity in the warp or weft. The difference in elasticity will cause the fabric to recover inconsistently after stretching or pressure, and become loose and lose its shape. Especially after denim fabrics are made into clothing, areas of clothing that are often stretched, such as the knees or elbows, are prone to permanent wrinkles or loss of elasticity. In addition, the organizational structure of the twill fabric itself increases the complexity of friction and tension distribution between fibers. Coupled with the presence of elastic fibers, tension control becomes more difficult.

[0057] In some specific embodiments, the pre-shrinking temperature is 170° C.-200° C. After the fabric is woven, the fabric is pre-shrinked to reduce the shrinkage rate of the fiber during use.

[0058] In some preferred embodiments, the spandex fiber is a pre-tensioned spandex fiber.

[0059] In some preferred embodiments, the tension spandex fiber is obtained by applying 10%-16% tension to spandex.

[0060] The present invention applies appropriate tension to the fibers during the spinning or weaving process to ensure that the fibers remain stable during the spinning, weaving and shaping processes, thereby avoiding problems such as shrinkage and excessive rebound in subsequent production or use, and improving the elasticity, durability and dimensional stability of spandex blended fabrics.

[0061] In some preferred embodiments, the preshrinking method is at least one of a mechanical preshrinking method, a steam preshrinking method, and a heat setting preshrinking method.

[0062] In some specific embodiments, the pre-shrinking temperature is 170°C-200°C.

[0063] In some specific embodiments of the core-spun yarn structure of the present invention, due to the different characteristics of spandex fiber, modified cotton fiber and polyester fiber, the preshrinkage process needs to take into account the shrinkage difference of various types of fibers, so the preshrinkage temperature is preferably 170°C-180°C.

[0064] Different fibers have different abilities to absorb dyes. Modified cotton fibers are easy to dye and have good dyeing uniformity, while polyester fibers and spandex fibers are not easy to dye. The structure of twill fabrics causes differences in the exposed surfaces of the fibers during the dyeing process, and the use of conventional dyeing methods will result in uneven dyeing, forming a "yin-yang side" or color difference. The present invention adopts a core-spun yarn structure and tightly wraps the twisted mixed fibers to overcome the problem of needing to dye spandex. The low-temperature dyeing process of disperse dyes can ensure that modified cotton fibers and polyester fibers have good dyeing uniformity.

[0065] In some preferred embodiments, the dyeing step is as follows:

[0066] The fabric is put into disperse dye for dyeing, and the liquid is drained after dyeing is completed. The fabric is washed with clean water to complete the dyeing. The dyeing temperature is preferably 70°C-85°C, and the dyeing time is preferably 20-40min.

[0067] In some preferred embodiments, a color fixing treatment is performed after dyeing, and the steps are as follows:

[0068] The dyed fabric is soaked in hot water and then drained, the hot water temperature is 50℃-60℃, the soaking time is 10-30min, and then a treatment solution containing 2.0-3.0% owf of acidic color fixing agent and pH 4.5 is used for color fixing treatment. After cooling, the liquid is drained and the fabric is washed out in clean water to complete the color fixing treatment. The preferred color fixing treatment temperature is 70℃-75℃, the color fixing treatment time is 10-30min, and the preferred cooling rate is 2.0℃ / min.

[0069] The technical solutions in the implementation cases of this application are described clearly and completely below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of invention protection. In the following embodiments, all raw materials are commercially available.

[0070] Example 1

[0071] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0072] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0073] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0074] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0075] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0076] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0077] Example 2

[0078] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 60% modified cotton fiber, 30% polyester fiber, and 10% spandex fiber.

[0079] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0080] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0081] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, to form a coating layer mixed fiber.

[0082] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0083] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 10 minutes. Then, it is fixed with a treatment solution containing 3.0% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 70°C, the color fixing treatment time is 30 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0084] Example 3

[0085] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 50% modified cotton fiber, 30% polyester fiber, and 20% spandex fiber.

[0086] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0087] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0088] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, to form a coating layer mixed fiber.

[0089] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0090] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 50°C and the soaking time is 30 minutes. Then, it is fixed with a treatment solution containing 2.0% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 20 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0091] Example 4

[0092] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0093] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0094] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L, the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and the concentration of citric acid was 10 g / L. Cotton fiber was immersed in the treatment solution for 1 hour, then dried, and baked at 120° C. for 10 minutes to obtain modified cotton fiber;

[0095] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0096] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0097] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0098] Comparative Example 1

[0099] This comparative example discloses a denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 50% modified cotton fiber, 30% polyester fiber, and 20% spandex fiber.

[0100] A method for preparing a denim fabric, comprising the following steps:

[0101] S1. Preparation of mixed fiber: cotton fiber and polyester fiber are taken out in proportion, mixed and sent into a spinning machine for spinning. During the spinning process, the fiber is cut and drawn into yarn, and the yarn is twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0102] S2, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S1 to obtain the wear-resistant core-spun yarn;

[0103] S3. Preparation of wear-resistant denim fabric: The wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 50°C and the soaking time is 30 minutes. Then, it is fixed with a treatment solution containing 2.0% owf of an acidic color fixing agent and a pH of 4.5. The liquid is drained after cooling, and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 20 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0104] Comparative Example 2

[0105] This comparative example discloses a denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% of modified cotton fiber, 20% of polyester fiber, and 10% of spandex fiber.

[0106] A method for preparing a denim fabric, comprising the following steps:

[0107] S1. Preparation of modified cotton fiber: chitosan was added into water to prepare a treatment solution, the chitosan concentration was 10 g / L, cotton fiber was immersed in the treatment solution for 2 h, then dried, and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0108] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0109] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0110] S4, preparation of denim fabric: the core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the denim fabric is obtained.

[0111] Comparative Example 3

[0112] This comparative example discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% of modified cotton fiber, 20% of polyester fiber, and 10% of spandex fiber.

[0113] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0114] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0115] S2. Preparation of mixed fiber: taking out modified cotton fiber and polyester fiber in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and pulled into yarns. The yarns are twisted to 6T / cm, and the twist direction is Z twist to form mixed fiber.

[0116] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0117] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with ordinary dyes at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0118] According to GB / T21196.3 "Determination of the abrasion resistance of textiles by the Martindale method - Part 3 - Determination of mass loss", the sample size is a circle with a diameter of 38 mm, the load is 9 KPa, the friction is 600 revolutions, and the mass loss rate is recorded. The test results of the abrasion resistance of the fabric and its color effect are shown in Table 1.

[0119] Table 1 Fabric abrasion resistance test results and color effects

[0120] sample Wear weight loss rate / % Dyeing effect Example 1 0.30±0.02c Even dyeing, no color difference Example 2 0.29±0.01cd Even dyeing, no color difference Example 3 0.27±0.01d Even dyeing, no color difference Example 4 0.27±0.01d Even dyeing, no color difference Comparative Example 1 0.39±0.02a Even dyeing, no color difference Comparative Example 2 0.36±0.02b Even dyeing, no color difference Comparative Example 3 0.29±0.01cd Uneven dyeing, lighter color, polyester fiber hardly dyes

[0121] Example 5

[0122] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0123] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0124] S1. Preparation of modified cotton fiber: chitosan and γ-aminopropyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-aminopropyltrimethoxysilane was 8 g / L, and the cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0125] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0126] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0127] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 180°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0128] Example 6

[0129] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0130] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0131] S1. Preparation of modified cotton fiber: chitosan and diethylenetriaminepropyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of diethylenetriaminepropyltrimethoxysilane was 8 g / L, and the cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0132] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a degree of 5 T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0133] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0134] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0135] Example 7

[0136] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0137] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0138] S1. Preparation of modified cotton fiber: chitosan and N-β (aminoethyl) -γ-aminopropyl triethoxysilane were added to water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of N-β (aminoethyl) -γ-aminopropyl triethoxysilane was 8 g / L. Cotton fiber was immersed in the treatment solution for 2 h, then dried, and baked at 120° C. for 10 min to obtain modified cotton fiber.

[0139] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 8 T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0140] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0141] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0142] Example 8

[0143] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0144] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0145] S1. Preparation of modified cotton fiber: chitosan and γ-methacryloxypropyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-methacryloxypropyltrimethoxysilane was 8 g / L, and the cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0146] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0147] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0148] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 2 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0149] Example 9

[0150] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 10 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0151] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0152] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0153] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0154] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0155] S4. Preparation of wear-resistant denim fabric: The wear-resistant core-spun yarn obtained in S3 is woven in 2 / 3 reinforced twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0156] Example 10

[0157] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 6 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0158] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0159] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0160] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0161] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0162] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0163] Embodiment 11

[0164] This embodiment discloses a wear-resistant denim fabric with a warp and weft density of 8 oz, which is composed of the following raw materials in percentage by mass: 70% modified cotton fiber, 20% polyester fiber, and 10% spandex fiber.

[0165] A method for preparing a wear-resistant denim fabric, comprising the following steps:

[0166] S1. Preparation of modified cotton fiber: chitosan and γ-(methacryloyloxy)propyltrimethoxysilane were added into water to prepare a treatment solution, wherein the concentration of chitosan was 10 g / L and the concentration of γ-(methacryloyloxy)propyltrimethoxysilane was 8 g / L, and cotton fiber was immersed in the treatment solution for 2 h, then dried and baked at 120° C. for 10 min to obtain modified cotton fiber;

[0167] S2, preparation of mixed fiber: taking out the modified cotton fiber and polyester fiber prepared in step S1 in proportion, mixing them and sending them into a spinning machine for spinning. During the spinning process, the fibers are cut and drawn into yarns, and the yarns are twisted with a twist of 6T / cm, and the twist direction is Z twist, so as to form a coating layer mixed fiber;

[0168] S3, preparation of core-spun yarn: covering the outer side of the spandex fiber with the coating layer mixed fiber prepared in step S2 to obtain the wear-resistant core-spun yarn;

[0169] S4, preparation of wear-resistant denim fabric: the wear-resistant core-spun yarn obtained in S3 is woven in 3 / 1 twill, pre-shrunk at 170°C, and dyed with disperse dye at 70°C for 40 minutes. The dyed fabric is soaked in hot water and drained. The hot water temperature is 60°C and the soaking time is 20 minutes. Then, it is fixed with a treatment solution containing 2.5% owf of an acidic color fixing agent and a pH of 4.5. After cooling, the liquid is drained and the fabric is washed in clean water to complete the color fixing treatment. The color fixing treatment temperature is 75°C, the color fixing treatment time is 25 minutes, and the cooling rate is 2.0°C / min. After finalization, the wear-resistant denim fabric is obtained.

[0170] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A wear-resistant denim fabric, characterized in that: The wear-resistant denim fabric is prepared by core-spun yarn with spandex fiber as the inner core and modified cotton fiber and polyester fiber blended mixed fiber as the covering layer through twill weaving, pre-shrinking, dyeing and shaping.

2. The wear-resistant denim fabric according to claim 1, characterized in that: The wear-resistant denim fabric comprises the following raw materials in percentage by mass: 50%-70% of modified cotton fiber, 20%-30% of polyester fiber, and 5%-20% of spandex fiber.

3. The wear-resistant denim fabric according to claim 2, characterized in that: The wear-resistant denim fabric comprises the following raw materials in percentage by mass: 70% of modified cotton fiber, 20% of polyester fiber and 10% of spandex fiber.

4. The wear-resistant denim fabric according to claim 2, characterized in that: The wear-resistant denim fabric comprises the following raw materials in percentage by mass: 60% of modified cotton fiber, 30% of polyester fiber and 10% of spandex fiber.

5. The wear-resistant denim fabric according to claim 2, characterized in that: The wear-resistant denim fabric comprises the following raw materials in percentage by mass: 50% of modified cotton fiber, 30% of polyester fiber and 20% of spandex fiber.

6. The wear-resistant denim fabric according to claim 1, characterized in that: The warp and weft density of the wear-resistant denim fabric is 6-10 oz.

7. The wear-resistant denim fabric according to claim 1, characterized in that: The modified cotton fiber is prepared by modifying cotton fiber with chitosan and a silane coupling agent.

8. The method for preparing the wear-resistant denim fabric according to any one of claims 1 to 7, characterized in that: The following steps are involved: The modified cotton fiber and the polyester fiber are spun and twisted to form a coating layer mixed fiber; the coating layer mixed fiber is coated on the outside of the spandex fiber to obtain a wear-resistant core-spun yarn, and the wear-resistant core-spun yarn is twill-woven, pre-shrunk, dyed and shaped to obtain a wear-resistant denim fabric.

9. The preparation method according to claim 1, characterized in that: The warp yarn density in the twill weaving is 27-32 yarns / cm, the weft yarn density is 13-20 yarns / cm, and the weaving is performed according to 3 / 1 twill, 2 / 1 twill or 2 / 3 reinforced twill variable twill structure.

10. The preparation method according to claim 1, characterized in that: The dyeing is low-temperature dyeing, and the dye is a disperse dye.

Citation Information

Patent Citations

  • Formaldehyde-free high-wear-resistance children anti-skid quilted socks

    CN113439889A

  • Multi-component fiber jean fabric and production process thereof

    CN115354435A

  • Environment-friendly flame-retardant polyester yarn and preparation method thereof

    CN115506062A

  • Wear-resistant fabric and preparation method thereof

    CN117535987A

  • Multi-component yarn and production method of jean fabric woven by same

    CN117987976A