Weft knitting fabric with anti-pilling and air inducing performance and processing method thereof

A weft-knitted fabric combining polyester and nylon with nano-silica and nano-silver treatments addresses wear resistance, microbial issues, and pilling, achieving enhanced durability and comfort for sportswear.

CN119061569AInactive Publication Date: 2024-12-03JIANGSU XINKAISHENG ENTERPRISE DEV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411420771.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional weft knitted fabrics face issues with insufficient wear resistance and mechanical strength, microbial activity, odor, pilling, and poor treatment efficiency, particularly in high-intensity activities and harsh environments.

Method used

A weft-knitted fabric composed of 75% polyester and 25% nylon fibers, treated with a mixture of nano-silica and nano-silver, and processed through co-spinning, weaving, nano-treatment, enzyme treatment, and heat curing, with specific conditions for enzyme and softening treatments to enhance durability and softness.

Benefits of technology

The fabric exhibits improved wear resistance, antimicrobial properties, reduced pilling, and enhanced softness, making it suitable for sportswear and other applications, with increased durability and comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061569A_ABST
    Figure CN119061569A_ABST
Patent Text Reader

Abstract

The invention relates to the field of textile materials, and discloses a weft knitting fabric with anti-pilling and air inducing performance and a processing method thereof.The fabric is composed of polyester fibers accounting for 75% of the total weight of the fabric and nylon fibers accounting for 25% of the total weight of the fabric; the total weight of the mixture of the nano silica and the nano silver contained in the fabric accounts for 1% of the total weight of the fabric, the nano silica accounts for 0.8%, and the nano silver accounts for 0.2%; the mixture is uniformly distributed with polyester and nylon fibers through a physical mixing process. The wear resistance and the mechanical strength of the fabric are remarkably enhanced by combining a bi-component fiber structure of polyester and nylon, so that the fabric shows excellent durability when being frequently washed and worn for a long time. The structure is particularly suitable for manufacturing sportswear subjected to high-intensity activities and severe environment tests, and meanwhile, the antimicrobial activity and the anti-pilling performance of the fabric are effectively improved by adding the compound of the nano silica and the nano silver.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile materials, in particular to a weft-knitted fabric with anti-pilling and air-inducing properties and a processing method thereof. Background Art

[0002] Weft knitted fabrics are widely used in the manufacture of daily clothing and sportswear due to their structural flexibility and adaptability to a wide range of application requirements. However, traditional weft knitted fabrics face several performance limitations in high-intensity activities and harsh environments:

[0003] Insufficient wear resistance and mechanical strength: Conventional weft knitted fabrics are usually made of a single fiber such as polyester or nylon. Although these single materials have certain strength or elasticity, they often show rapid wear, tear and aging after repeated washing and long-term wear. Especially in outdoor sports or other sports activities that require extreme durability, the performance of these fabrics is relatively insufficient.

[0004] Microbial activity and odor issues: Existing fabrics are often not adequately treated with antimicrobial agents when worn for long periods of time in a closed, humid environment, which can easily lead to the growth of bacteria and fungi, resulting in unpleasant odors and reduced comfort and health for the wearer.

[0005] Pilling and softness issues: Pilling is a common defect in weft knitted fabrics, especially in low-cost and untreated fabrics. Pilling not only affects the aesthetics of the fabric, but also reduces the comfort of wearing. In addition, the rigidity and roughness of the fabric often greatly reduce the wearing experience.

[0006] Poor treatment efficiency and effect: Traditional fabric processing methods, such as softening and enzyme treatment, often lack precise condition control, such as humidity adjustment and temperature control, which leads to fluctuations in treatment results and cannot effectively improve fabric performance in a long-term manner, especially in large-scale production.

[0007] Therefore, the present invention provides a weft-knitted fabric with anti-pilling and air-inducing properties and a processing method thereof to solve the deficiencies of the prior art. Summary of the invention

[0008] In view of the deficiencies of the prior art, the present invention provides a weft-knitted fabric with anti-pilling and air-inducing properties and a processing method thereof, aiming to improve the wear resistance, antimicrobial properties, softness and overall durability of the fabric in sportswear and other applications.

[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions: a weft knitted fabric, the fabric is composed of the following components:

[0010] Polyester fiber accounts for 75% of the total weight of the fabric, and nylon fiber accounts for 25% of the total weight;

[0011] The mixture of nano-silica and nano-silver contained in the fabric accounts for 1% of the total weight of the fabric, of which nano-silica accounts for 0.8% and nano-silver accounts for 0.2%;

[0012] The mixture is evenly distributed with the polyester and nylon fibers through a physical mixing process.

[0013] Preferably, the average particle size of the nano-silica and nano-silver particles ranges from 10 to 100 nanometers to ensure their uniform distribution in the fiber and surface attachment.

[0014] Preferably, the processing method of weft knitted fabric comprises the following steps:

[0015] The polyester and nylon fibers were co-spun into bicomponent fibers at a weight ratio of 75:25 by co-spinning technology;

[0016] The bicomponent fibers are woven into weft-knitted fabrics using a weaving machine, and the weft density is controlled to be 40-60 fibers per inch during the weaving process;

[0017] The woven fabric is immersed in an aqueous solution containing 0.8% nano-silicon and 0.2% nano-silver for 24-28 hours, and the solution temperature is maintained at 25°C;

[0018] After soaking, the fabric was heat treated at 150 °C for 60 min to solidify the nanoparticles.

[0019] Preferably, the polyester core and the polyethylene sheath of the bicomponent fiber form a core / sheath structure, wherein the polyethylene sheath accounts for 30% of the total fiber diameter.

[0020] Preferably, the immersion treatment of the nanoparticles is carried out at room temperature for 24-28 hours.

[0021] Preferably, a treatment method for improving the softness and anti-pilling properties of weft knitted fabrics comprises the following steps:

[0022] Treat fabrics with cellulase enzymes specific for polyester and nylon;

[0023] The enzyme treatment was carried out at pH 5.5 and temperature 55°C;

[0024] The enzyme treatment time is 1-1.2 hours;

[0025] The enzyme treatment is followed by a thorough cleaning and neutralization to remove all unreacted enzymes and ensure fabric stability.

[0026] Preferably, before the cellulase treatment step, the fabric is pretreated to adjust the moisture content of the fabric to an appropriate level, wherein the pretreatment comprises soaking the fabric in an aqueous solution containing 0.1%-0.2% of a surfactant for 15-20 minutes, followed by light rolling and dehydration to adjust the moisture content of the fabric to 60%-70%.

[0027] Preferably, after the cellulase treatment step, the fabric is subjected to a special softening treatment, and the softener used in the softening treatment step is a cationic softener, and the amount used is 0.5%-1% of the weight of the fabric. The softening treatment is carried out at a temperature of 60°C-70°C and lasts for 30-45 minutes.

[0028] Preferably, the weft knitted fabric is used to make running, hiking and other high intensity sports activities clothing applications.

[0029] The present invention provides a weft-knitted fabric with anti-pilling and air-inducing properties and a processing method thereof.

[0030] Beneficial effects:

[0031] 1. The present invention significantly enhances the wear resistance and mechanical strength of the fabric by combining a bicomponent fiber structure of polyester and nylon. Polyester provides high wear resistance, while nylon increases elasticity and tear resistance, making the fabric of the present invention show excellent durability in frequent washing and long-term wear. This structure is particularly suitable for manufacturing sportswear that withstands high-intensity activities and harsh environments.

[0032] 2. The present invention effectively improves the antimicrobial activity and anti-pilling performance of the fabric by adding a composite of nano-silicon and nano-silver. The antibacterial properties of nano-silver help prevent bacterial growth and odor generation, enhancing the hygienic safety of the fabric. At the same time, the protective layer formed by nano-silicon on the fiber surface effectively resists wear and tear during daily wear, reduces pilling, and prolongs the life of clothing.

[0033] 3. Specific cellulase treatment optimizes the softness of the fabric, making it more suitable for wearing directly against the skin. By decomposing the extra tiny fibers on the surface of the fabric, the present invention not only improves the feel of the fabric, but also reduces pilling, allowing users to feel more comfortable and free when moving.

[0034] 4. The fabric of the present invention undergoes a specific pretreatment before the cellulase treatment to adjust the humidity to the optimal level to ensure the maximum effect of the enzyme. The surfactant added in the pretreatment further promotes the uniform distribution of moisture, creating ideal conditions for enzyme treatment. The subsequent cationic softening treatment increases the softness of the fabric while improving the antistatic performance and overall wearing experience of the fabric. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1This is a flow chart of the processing method of weft knitted fabrics. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings of the present invention specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Please see attached Figure 1 :

[0038] Example:

[0039] Embodiment 1: manufacture weft-knitted fabric for outdoor sportswear

[0040] Implementation steps:

[0041] Fiber selection and ratio: Use a mixture of 75% polyester and 25% nylon to spin a bicomponent fiber, and use co-spinning technology to ensure a uniform blend of the two fibers to improve the overall durability and mechanical strength of the fabric.

[0042] Weaving process: Use a weaving machine to weave the two-component fiber into a weft-knitted fabric, and control the weft density to 50 fibers per inch. This density setting helps to improve the tear resistance of the fabric and adapt to the complex environment of outdoor sports.

[0043] Nano treatment: The fabric is soaked in a solution containing 0.8% nano-silica and 0.2% nano-silver for 24 hours at 25°C to ensure that the nanoparticles are evenly attached to the fibers, enhancing the antimicrobial activity and reducing pilling.

[0044] Heat treatment curing: The fabric is heat treated at 150°C for 60 minutes to cure the nanoparticles, ensuring durability and long-term antibacterial properties of the fabric.

[0045] Summary of the embodiment: The fabric in this embodiment is particularly suitable for outdoor sportswear. Its wear resistance and antibacterial properties enable it to maintain high performance during long-term outdoor activities, reduce maintenance frequency, and increase service life.

[0046] Embodiment 2: manufacture weft-knitted fabrics for high-end sports yoga clothing

[0047] Implementation steps:

[0048] Fiber selection and ratio: The fibers are co-spun in a ratio of 75% polyester and 25% nylon to ensure that the fabric has good elasticity and resilience, suitable for the needs of yoga wear.

[0049] Weaving process: Woven on a loom with a controlled weft density of 60 fibers per inch, which helps increase the softness and breathability of the fabric, making it more comfortable when stretched.

[0050] Nano-treatment: The fabric is soaked in a specially formulated nano-treatment solution for 28 hours at a controlled temperature of 25°C to ensure deep penetration and even distribution of the nanoparticles.

[0051] Heat treatment curing: After soaking, the fabric is heat treated at 150°C for 60 minutes to enhance the bonding strength between the nanoparticles and the fibers, and improve the durability and functionality of the fabric.

[0052] Summary of the embodiment: The softness and antibacterial properties of the fabric make it very suitable for high-end yoga clothing, which can provide good support while ensuring hygiene and comfort.

[0053] Embodiment 3: manufacture weft-knitted fabric for professional-grade bicycle racing uniform

[0054] Implementation steps:

[0055] Fiber selection and ratio: 75% polyester and 25% nylon blended to provide the necessary wear resistance and moderate elasticity for cycling uniforms.

[0056] Weaving technology: The weft density is adjusted to 55 fibers per inch during weaving to balance the strength and breathability of the fabric to adapt to the friction and heat dissipation generated by high-speed riding.

[0057] Nanomaterial treatment: Soak the fabric in a mixed solution of nano-silica and nano-silver for 26 hours, with the temperature controlled at 25°C to achieve the best nanoparticle adsorption effect.

[0058] Heat treatment curing: The fabric is heat treated at 150°C for 60 minutes to ensure the long-term binding of the nanoparticles and the antibacterial and anti-wear properties of the fabric.

[0059] Summary of the embodiment: This fabric has high air permeability and quick-drying properties, providing an excellent wearing experience for professional cyclists while ensuring stable performance during competitions.

[0060] Embodiment 4: manufacture weft-knitted fabric for children's outdoor wear

[0061] Implementation steps:

[0062] Fiber Ratio and Weaving: The fibers are spun in a blend of 75% polyester and 25% nylon, and the weft density is adjusted to 40 threads per inch during weaving to enhance the softness and adaptability of the fabric, especially suitable for active children.

[0063] Nano treatment and soaking: The fabric was soaked in a solution containing 0.8% nano silica and 0.2% nano silver for 24 hours at 25°C to enhance the antibacterial and wear resistance of the fabric.

[0064] Heat treatment: After soaking, heat treatment is carried out at 150℃ for 60 minutes. The curing treatment improves the durability of the fabric.

[0065] Summary of the embodiment: The fabric of this embodiment ensures the safety and comfort of children during outdoor activities by enhancing antibacterial properties and softness. The fabric is durable and easy to clean and maintain.

[0066] Example 5: Manufacturing weft-knitted fabrics for business casual wear

[0067] Implementation steps:

[0068] Fiber preparation and weaving: Polyester and nylon are co-spun in a ratio of 75:25, and the weft density is adjusted to 60 threads per inch to improve the overall smoothness and appearance texture of the fabric.

[0069] Nano solution treatment: The fabric is immersed in nano-silica and nano-silver solution for 28 hours at 25°C to ensure uniform coverage of the nanoparticles.

[0070] Heat treatment: After soaking, the fabric is heat treated at 150°C for 60 minutes to solidify the nanoparticles and enhance the functional characteristics of the fabric.

[0071] Summary of the embodiment: The fabric of this embodiment is suitable for business casual wear. Its antibacterial property and low maintenance requirement make it an ideal daily wear choice for business people while maintaining an elegant appearance and a comfortable wearing experience.

[0072] Summary:

[0073] These five embodiments demonstrate the versatility and high performance of the fabrics of the present invention in different application scenarios. Through fine fiber selection, application of nanotechnology and precise processing technology, the durability, antibacterial property, softness and overall performance of the fabrics are effectively improved, meeting a wide range of needs from outdoor sports to business leisure.

[0074] Comparative experiment:

[0075] Experiment 1: Wear resistance comparison experiment

[0076] Purpose: To verify the superiority of the weft-knitted fabric of the present invention over the prior art (standard single fiber fabric) in terms of wear resistance.

[0077] Technical solution composition:

[0078] The solution of the present invention is: 75% polyester and 25% nylon are blended, and a mixture of 0.8% nano silica and 0.2% nano silver is added.

[0079] Existing technical solution: Use 100% polyester fabric without any nano material reinforcement.

[0080] Experimental setup:

[0081] Test equipment: Martindale abrasion tester was used according to ASTM D4966.

[0082] Test conditions: 10,000 friction cycles, each sample tested under a load of 500 g.

[0083] Evaluation parameters: Record the mass change, fiber damage rate and structural changes under the microscope for each sample.

[0084] Data table:

[0085]

[0086] Experiment 2: Antibacterial performance comparison experiment

[0087] Objective: To demonstrate the significant difference in antibacterial properties between the blended fabric treated with nanosilver and the untreated pure polyester fabric.

[0088] Technical solution composition:

[0089] The solution of the present invention: 75% polyester + 25% nylon, with 0.2% nano silver added.

[0090] Existing technical solution: 100% polyester fabric, without antimicrobial additives.

[0091] Experimental setup:

[0092] Test standard: Antimicrobial activity was evaluated in accordance with ISO 20743.

[0093] Inoculated strain: Staphylococcus aureus.

[0094] Test duration: Bacteria reduction rate within 24 hours.

[0095] Data table:

[0096] Material Type Antimicrobial additives Bacteria reduction rate (%) Fabric of the present invention have 0.995 Existing technical fabrics none 0.05

[0097] Experiment 3: Softness Test

[0098] Objective: To prove that the blended fabric of the present invention treated with cellulase is softer than the pure polyester fabric treated with conventional softener.

[0099] Technical solution composition:

[0100] The solution of the present invention: 75% polyester and 25% nylon are treated with cellulase.

[0101] Existing technical solution: pure polyester fabric, traditional softener treatment.

[0102] Experimental setup:

[0103] Test Equipment: The compression softness of fabrics was measured using the Kawabata evaluation system.

[0104] Evaluation parameters: Softness value and surface touch score were recorded.

[0105] Data table:

[0106]

[0107]

[0108] Experiment 4: Processing efficiency comparison experiment

[0109] Objective: To demonstrate that the integrated treatment method (nano and enzyme treatment) of the present invention is superior to the traditional pure poly-chou fabric treated in steps in terms of production efficiency.

[0110] Technical solution composition:

[0111] The scheme of the present invention: polyester nylon blended fabric treated with comprehensive nanometer and enzyme.

[0112] Existing technical solution: pure polyester fabric, softener and antibacterial treatment respectively.

[0113] Experimental setup:

[0114] Evaluation parameters: total processing time, energy consumption, water consumption.

[0115] Data table:

[0116]

[0117] Summary:

[0118] These experimental results clearly demonstrate the significant improvements of the present invention in terms of wear resistance, antibacterial properties, softness and processing efficiency compared to the prior art. By integrating nanotechnology and bio-enzyme treatment, the present invention not only improves the performance of the fabric, but also significantly improves production efficiency by reducing processing steps and consumption. The technical solution of the present invention is fully disclosed, ensuring its creativity and practicality, and providing an effective solution in the modern textile industry.

[0119] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A weft knitted fabric, It is characterized in that The fabric is composed of the following components: Polyester fiber accounts for 75% of the total weight of the fabric, and nylon fiber accounts for 25% of the total weight; The mixture of nano-silica and nano-silver contained in the fabric accounts for 1% of the total weight of the fabric, of which nano-silica accounts for 0.8% and nano-silver accounts for 0.2%; The mixture is evenly distributed with the polyester and nylon fibers through a physical mixing process.

2. The weft knitted fabric according to claim 1, It is characterized in that The average particle size of the nano-silica and nano-silver particles ranges from 10 to 100 nanometers to ensure their uniform distribution in the fibers and surface attachment.

3. The method for processing a weft-knitted fabric according to any one of claims 1 to 2, It is characterized in that The following steps are involved: The polyester and nylon fibers were co-spun into bicomponent fibers at a weight ratio of 75:25 by co-spinning technology; The bicomponent fibers are woven into weft-knitted fabrics using a weaving machine, and the weft density is controlled to be 40-60 fibers per inch during the weaving process; The woven fabric is immersed in an aqueous solution containing 0.8% nano-silicon and 0.2% nano-silver for 24-28 hours, and the solution temperature is maintained at 25°C; After soaking, the fabric was heat treated at 150 °C for 60 min to solidify the nanoparticles.

4. The method for processing a weft-knitted fabric according to claim 3, It is characterized in that The polyester core of the bicomponent fiber and the polyethylene sheath form a core / sheath structure, wherein the polyethylene sheath accounts for 30% of the total fiber diameter.

5. The method for processing a weft-knitted fabric according to claim 3, It is characterized in that The immersion treatment of the nanoparticles is carried out at room temperature and lasts for 24-28 hours.

6. A method for improving the softness and anti-pilling properties of the weft-knitted fabric according to any one of claims 1 to 2, It is characterized in that The following steps are involved: Treat fabrics with cellulase enzymes specific for polyester and nylon; The enzyme treatment was carried out at pH 5.5 and temperature 55°C; The enzyme treatment time is 1-1.2 hours; The enzyme treatment is followed by a thorough cleaning and neutralization to remove all unreacted enzymes and ensure fabric stability.

7. The method for treating the softness and anti-pilling properties of weft knitted fabrics according to claim 6, It is characterized in that Before the cellulase treatment step, the fabric is pretreated to adjust the moisture content of the fabric to an appropriate level. The pretreatment includes soaking the fabric in an aqueous solution containing 0.1%-0.2% of a surfactant for 15-20 minutes, followed by light rolling and dehydration to adjust the moisture content of the fabric to 60%-70%.

8. The method for treating the softness and anti-pilling properties of weft knitted fabrics according to claim 6, It is characterized in that After the cellulase treatment step, the fabric is subjected to a special softening treatment. The softener used in the softening treatment step is a cationic softener, and the amount used is 0.5%-1% of the weight of the fabric. The softening treatment is carried out at a temperature of 60°C-70°C and lasts for 30-45 minutes.

9. Use of the weft-knitted fabric according to any one of claims 1 to 8 in manufacturing clothing for running, hiking and other high-intensity sports activities.

Citation Information

Patent Citations

  • Soft and comfortable novel compound polypropylene fiber fabric

    CN105088396A

  • Method of treating polyester textile

    CN107109780A

  • Super-hydrophobic antibacterial knitted fabric and preparation method thereof

    CN112195552A

  • Wear-resistant and anti-pilling antibacterial nano fabric and preparation method thereof

    CN113652862A

  • High-performance polyamide-polyester composite fiber and preparation method thereof

    CN118668325A