Carbon fiber glue spraying process
By pouring glue on the upper surface of carbon fiber soft felt and using negative pressure fan to penetrate glue, the problems of complex processes and poor penetration in the existing technology are solved, simplified process and efficient penetration are achieved, and the excess glue can be recovered, which improves production efficiency .
Patent Information
- Application Number
- CN202411153029.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-03
AI Technical Summary
The existing carbon fiber glue coating process is complex and time-consuming and labor-intensive. The resin glue cannot penetrate effectively into the soft felt, and the excess glue cannot be recovered.
Carbon fiber soft felt is conveyed through the conveyor belt, first evenly paint the glue on the upper surface, and then use negative pressure fan and grid curtain to penetrate the glue, eliminating the glue on the lower surface, simplifying the procedure and improving efficiency, and passing the flow control valve and speed regulation Motor adjusts speed and glue flow.
The glue and glue seepage are achieved in one-time conveying. The resin glue can effectively penetrate into the carbon fiber soft felt, simplifying the process flow, improving efficiency, and recycling the glue seepage through the arc-shaped slider to avoid blocking the negative pressure fan.
Smart Images

Figure CN119061599A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fiber glue spraying, and in particular to a carbon fiber glue spraying process. Background Art
[0002] After carbon fiber is produced, it is usually coated with a layer of resin glue on its surface to meet the process requirements of the subsequent curing process. The existing coating methods are double-sided coating, that is, coating the upper surface with glue and then turning it over, coating the lower surface again or coating the upper and lower surfaces with glue at the same time through a steering roller.
[0003] However, this glue pouring process requires continuous turning, and the glue just poured is very wet and easy to flow and aggregate, resulting in an uneven pouring surface or dripping, wasting glue and polluting the environment; at the same time, the resin glue has a certain viscosity, and the naturally flowing resin glue cannot penetrate well into the soft felt. Summary of the invention
[0004] The main purpose of the present invention is to provide a carbon fiber glue pouring process, aiming to solve the technical problems that the prior art is not only complicated in procedure, time-consuming and labor-intensive, but also that the poured resin glue cannot be effectively controlled and well penetrated into the interior of the carbon fiber soft felt, and the excess glue cannot be recovered.
[0005] To achieve the above object, the present invention provides a carbon fiber glue coating process, comprising: Step 1: Carbon fiber soft felt input; The un-glued carbon fiber soft felt is placed flatly on the input conveyor belt and transported to the bottom of the glue spraying head; the driving pulley of the conveyor belt is equipped with an input speed regulating motor, and the input speed is adjusted by the input speed regulating motor; Step 2: Apply glue to the upper surface of the carbon fiber soft felt; The input carbon fiber soft felt is evenly coated with resin glue on its upper surface through a glue spraying head; the glue spraying head is connected to an external glue storage tank through a glue spraying pipe, and a flow control valve is installed on the glue spraying pipe, and the glue spraying amount is controlled by the flow control valve; Step 3: Glue infiltration into carbon fiber soft felt; The carbon fiber soft felt after the upper surface is coated with glue passes through a negative pressure fan, and negative pressure glue penetration is carried out below it; the glue penetration is completed through a mesh curtain and a negative pressure fan, the mesh curtain is flush with the input conveyor belt, and the negative pressure fan is arranged below the mesh curtain. When the carbon fiber soft felt after the upper surface is coated with glue passes through the mesh curtain, the negative pressure fan is started to allow the resin glue on the upper surface to fully penetrate into the interior of the carbon fiber soft felt.
[0006] Step 4: Output the carbon fiber soft felt after infiltration; The carbon fiber soft felt after the infiltration of glue is output through an output conveyor belt, and an output speed regulating motor is installed on the driving pulley of the output conveyor belt.
[0007] Furthermore, the thickness of the carbon fiber soft felt is consistent with the thickness of the glue pouring, both of which are 10 mm; The input speed is consistent with the output speed, which is 0.15m / s-0.19m / s.
[0008] Furthermore, the flow rate of the flow control valve in step 3 is: 7m 3 / h- 9m 3 / h, the negative pressure is: 5300pa.
[0009] Furthermore, the grid curtain is installed on the glue storage groove, and an upper slide plate and a lower slide plate are provided on both sides of the glue storage groove. The upper slide plate and the lower slide plate are both arc-shaped, and a gap is provided between the upper slide plate and the lower slide plate, which is used for the negative pressure fan to form negative pressure under the glue storage groove and slide out the seeped glue at the same time.
[0010] Furthermore, the negative pressure fan is installed on both sides of the upper slide plate and the lower slide plate through a negative pressure pipe.
[0011] Furthermore, a glue receiving hopper is provided at the bottom of the glue storage tank.
[0012] Furthermore, the glue spraying head is installed above the mesh curtain through a supporting frame.
[0013] The beneficial effects of the present invention are embodied in: In the present invention, the carbon fiber soft felt is transported by a conveyor belt to be mobile glue-coated, and the carbon fiber soft felt with glue coated on the upper surface is subjected to negative pressure glue penetration on the lower surface through a mesh curtain, and the glue coating and glue penetration can be completed in one transportation, and the glue coating on the upper surface can penetrate into the interior and the lower surface, eliminating the glue coating on the lower surface, simplifying the procedure, and improving efficiency; The input and output speed or glue flow control valve can be adjusted according to the glue seepage situation, with strong controllability; The seeped glue slides out through the upper and lower slide plates and can be recycled and utilized repeatedly. The arc-shaped upper and lower slide plates are arranged at intervals to prevent the seeped glue from clogging the negative pressure fan. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a schematic diagram of the three-dimensional structure of the present invention; Figure 2 It is a schematic diagram of the structure of the glue penetration mechanism of the present invention; Figure 3 for Figure 2 Front view of .
[0015] Description of reference numerals: 101, input conveyor belt, 102, input speed regulating motor, 103, output conveyor belt, 104, output speed regulating motor; 201, glue spraying head, 202, flow control valve, 203, support frame, 204, glue spraying tube; 301. Grid curtain, 302. Glue storage tank, 303. Negative pressure pipe, 304. Negative pressure fan, 305. Glue receiving hopper, 306. Upper slide plate, 307. Lower slide plate. DETAILED DESCRIPTION
[0016] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. In the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other.
[0017] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative work shall fall within the scope of protection of the present invention.
[0018] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0019] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0020] In addition, the meaning of "and / or" in the whole text includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, "plurality" means more than two.
[0021] In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist.
[0022] Embodiment 1
[0023] See also Figures 1 to 3 , a carbon fiber glue coating process, comprising: Step 1: Carbon fiber soft felt input; The un-glued carbon fiber felt is placed flatly on the input conveyor belt 101 and transported to the bottom of the glue spraying head 201; the driving pulley of the conveyor belt 101 is equipped with an input speed regulating motor 102, and the input speed is adjusted by the input speed regulating motor 102; Step 2: Apply glue to the upper surface of the carbon fiber soft felt; The input carbon fiber soft felt is evenly coated with resin glue on its upper surface through a glue spraying head 201; the glue spraying head 201 is connected to an external glue storage tank through a glue spraying pipe 204, and a flow control valve 202 is installed on the glue spraying pipe 204, and the glue spraying amount is controlled by the flow control valve 202; Step 3: Glue infiltration into carbon fiber soft felt; The carbon fiber soft felt after the upper surface is coated with glue passes through a negative pressure fan, and negative pressure glue penetration is carried out below it; the glue penetration is completed through a mesh curtain 301 and a negative pressure fan 304, the mesh curtain 301 is flush with the input conveyor belt 101, and the negative pressure fan 304 is arranged below the mesh curtain 301. When the carbon fiber soft felt after the upper surface is coated with glue passes through the mesh curtain 301, the negative pressure fan 304 is started to allow the resin glue on the upper surface to fully penetrate into the interior of the carbon fiber soft felt.
[0024] Step 4: Output the carbon fiber soft felt after infiltration; The carbon fiber soft felt after the infiltration of glue is output through the output conveyor belt 103, and the output speed regulating motor 104 is installed on the driving pulley of the output conveyor belt 103.
[0025] The carbon fiber soft felt is transported by a conveyor belt for mobile glue spraying. The carbon fiber soft felt with glue sprayed on the upper surface is subjected to negative pressure glue penetration on the lower surface through a mesh curtain. The glue spraying and glue penetration can be completed in one transportation. The glue sprayed on the upper surface can penetrate into the interior and the lower surface, eliminating the glue spraying on the lower surface, simplifying the procedure and improving efficiency. The thickness of the carbon fiber soft felt is consistent with the thickness of the glue spraying, both of which are 10mm; The input speed is consistent with the output speed, which is 0.15 m / s.
[0026] The flow rate of the flow control valve 202 in step 3 is: 7m 3 / h, the negative pressure is: 5300pa.
[0027] The input and output speed or glue flow control valve can be adjusted according to the glue seepage situation, with strong controllability; The mesh curtain 301 is installed on the glue storage groove 302. An upper slide plate 306 and a lower slide plate 307 are arranged on both sides of the glue storage groove 302. The upper slide plate 306 and the lower slide plate 307 are both arc-shaped, and a gap is provided between the upper slide plate 306 and the lower slide plate 307 for the negative pressure fan 304 to form negative pressure under the glue storage groove 302 and slide out the seeped glue at the same time.
[0028] The negative pressure fan 304 is installed on both sides of the upper slide plate 306 and the lower slide plate 307 through the negative pressure pipe 303. The seeping glue slides out through the upper and lower slide plates and can be recycled and reused repeatedly. The arc-shaped upper and lower slide plates are arranged at intervals to prevent the seeping glue from blocking the negative pressure fan.
[0029] A glue receiving hopper 305 is provided at the bottom of the glue storage tank 302. The glue spraying head 201 is installed above the grid curtain 301 through a support frame 203.
[0030] Embodiment 2
[0031] The difference between this embodiment and embodiment 1 is that: The thickness of the carbon fiber soft felt is consistent with the thickness of the glue spraying, both of which are 10mm; The input speed is consistent with the output speed, which is 0.19 m / s.
[0032] In step three, the flow rate of the flow control valve 202 is: 9m3 / h, and the negative pressure is: 5300pa.
[0033] The input and output speed or glue flow control valve can be adjusted according to the glue seepage situation, with strong controllability; When changing the speed or the glue flow rate, the penetration conditions are shown in Table 1.
[0034] Soft felt thickness (mm) Glue coating thickness (mm) Input speed (m / s) <![CDATA[Flow rate (m 3 / h)]]> Negative pressure (pa) Output speed (m / s) Glue penetration depth (mm) 10 10 0.15 7 5300 0.15 10 10 10 0.19 9 5300 0.19 10 The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A carbon fiber glue coating process, characterized in that ,include: Step 1: Carbon fiber soft felt input; The un-glued carbon fiber soft felt is placed flatly on the input conveyor belt (101) and conveyed to the bottom of the glue spraying head (201); the driving pulley of the conveyor belt (101) is equipped with an input speed regulating motor (102), and the input speed is adjusted by the input speed regulating motor (102); Step 2: Apply glue to the upper surface of the carbon fiber soft felt; The input carbon fiber soft felt is evenly coated with resin glue on its upper surface through a glue spraying head (201); the glue spraying head (201) is connected to an external glue storage tank through a glue spraying pipe (204); a flow control valve (202) is installed on the glue spraying pipe (204); and the glue spraying amount is controlled by the flow control valve (202); Step 3: Glue infiltration into carbon fiber soft felt; The carbon fiber soft felt after the glue coating on the upper surface passes through a negative pressure fan, and negative pressure glue penetration is performed below the felt; the glue penetration is completed through a mesh curtain (301) and a negative pressure fan (304), the mesh curtain (301) is flush with the input conveyor belt (101), and the negative pressure fan (304) is arranged below the mesh curtain (301). When the carbon fiber soft felt after the glue coating on the upper surface passes through the mesh curtain (301), the negative pressure fan (304) is started to allow the resin glue on the upper surface to fully penetrate into the interior of the carbon fiber soft felt; Step 4: Output the carbon fiber soft felt after infiltration; The carbon fiber soft felt that has been infiltrated with glue is output via an output conveyor belt (103), and an output speed regulating motor (104) is mounted on a driving pulley of the output conveyor belt (103).
2. A carbon fiber glue coating process as claimed in claim 1, characterized in that: The thickness of the carbon fiber soft felt is consistent with the thickness of the glue spraying, both of which are 10mm; The input speed is consistent with the output speed, which is 0.15m / s-0.19m / s.
3. A carbon fiber glue coating process as claimed in claim 1, characterized in that: The flow rate of the flow control valve (202) in step 3 is: 7m 3 / h-9 m 3 / h, the negative pressure is: 5300pa.
4. A carbon fiber glue coating process as claimed in claim 1, characterized in that: The mesh curtain (301) is installed on the glue storage groove (302), and an upper slide plate (306) and a lower slide plate (307) are arranged on both sides of the glue storage groove (302). The upper slide plate (306) and the lower slide plate (307) are both arc-shaped, and a gap is provided between the upper slide plate (306) and the lower slide plate (307) for the negative pressure fan (304) to form negative pressure below the glue storage groove (302) and slide out the glue that has seeped out.
5. A carbon fiber glue coating process as claimed in claim 4, characterized in that: The negative pressure fan (304) is installed on both sides of the upper slide plate (306) and the lower slide plate (307) through the negative pressure pipe (303).
6. A carbon fiber glue coating process as claimed in claim 4, characterized in that: A glue receiving hopper (305) is provided at the bottom of the glue storage tank (302).
7. A carbon fiber glue coating process as claimed in claim 1, characterized in that: The glue spraying head (201) is installed above the mesh curtain (301) through a support frame (203).