Sizing agent and preparation method thereof, carbon fiber and composite material

By covalently connecting SiO2 epoxy resin and polyphenoloxy resin in the sizing agent, the interface bonding strength between carbon fiber and matrix resin is improved, the problem of insufficient binding performance after the carbon fiber sizing agent is solved, and the mechanics of composite materials are realized Performance improvement.

CN119061695AActive Publication Date: 2024-12-03ZHONGFU SHENYING CARBON FIBER

Patent Information

Application Number
CN202411350850.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03
Estimated Expiration
2044-09-26

AI Technical Summary

Technical Problem

The binding performance enhancement effect of existing carbon fiber sizing agents with matrix resin is limited, resulting in carbon fibers being easily bleached and loose during use and processing, affecting the mechanical properties of composite materials.

Method used

Using an emulsion-like sizing agent, by covalently connecting SiO2 to the epoxy resin, the roughness and active functional groups of the carbon fiber surface are increased, and the polyphenoloxy resin is combined with each other to form excellent silk removal smooth performance, reduce fiber bleeding, and improve carbon fiber Interface bonding strength with matrix resin.

Benefits of technology

The interface bonding strength between carbon fiber and matrix resin and the mechanical properties of composite materials are significantly improved, and the viscosity increase and processing difficulties caused by uneven dispersion of SiO2 are avoided, ensuring good bonding between carbon fiber and matrix resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061695A_ABST
    Figure CN119061695A_ABST
Patent Text Reader

Abstract

The invention provides a sizing agent and a preparation method thereof, a carbon fiber and a composite material, and belongs to the technical field of carbon fiber sizing agents. The sizing agent is in an emulsion state and comprises a main sizing agent and water, the main slurry comprises the following components in parts by weight: 20-30 parts of phenoxy resin, 10-20 parts of epoxy resin and 10-20 parts of an emulsifier; wherein SiO2 is covalently connected to the epoxy resin. The epoxy resin of the sizing agent is covalently connected with SiO2, so that the surface roughness of the carbon fiber treated by the sizing agent can be remarkably increased, the number of active functional groups on the surface of the carbon fiber treated by the sizing agent can be increased, the fiber fluffing amount of the carbon fiber treated by the sizing agent can be reduced, and the sizing agent has the advantages of high sizing agent utilization rate and high sizing agent utilization rate. Furthermore, the interface bonding strength between the carbon fiber treated by the sizing agent and the matrix resin can be improved, and the mechanical property of a composite material formed by the carbon fiber and the matrix resin can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of carbon fiber sizing agents, and in particular to a sizing agent and a preparation method thereof, carbon fibers and composite materials. Background Art

[0002] Carbon fiber is made from raw silk through a series of complex physical and chemical changes such as pre-oxidation, carbonization, and graphitization. Carbon fiber has low elongation and is relatively brittle. During use and processing, it will be stretched and rubbed, which will cause fluffing and looseness, seriously affecting the bonding performance between carbon fiber and matrix resin. Therefore, sizing treatment must be carried out in carbon fiber production. After sizing treatment, the bonding performance between carbon fiber and matrix resin will be enhanced.

[0003] However, the existing sizing agent-treated carbon fibers have limited effect in enhancing the bonding performance between the carbon fibers and the matrix resin. Summary of the invention

[0004] The purpose of the present application is to provide a sizing agent and a preparation method thereof, carbon fiber and a composite material, which are intended to improve the bonding performance between the carbon fiber treated with the sizing agent and the matrix resin.

[0005] In the first aspect, the present application provides a sizing agent, which is in the form of an emulsion and includes a main slurry and water; the main slurry includes the following components by weight: 20 to 30 parts of polyphenol oxide resin, 10 to 20 parts of epoxy resin and 10 to 20 parts of emulsifier; wherein SiO2 is covalently bonded to the epoxy resin.

[0006] The present application can not only significantly increase the surface roughness of the carbon fiber treated with the sizing agent by covalently linking SiO2 to the epoxy resin of the sizing agent, but also increase the number of active functional groups on the surface of the carbon fiber treated with the sizing agent, thereby improving the interfacial bonding strength between the carbon fiber treated with the sizing agent and the matrix resin, and improving the mechanical properties of the composite material formed by the carbon fiber and the matrix resin; compared with directly adding SiO2 to the sizing agent, covalently linking SiO2 to the epoxy resin is beneficial to avoid the problem of a sharp increase in the viscosity of the sizing agent and difficulty in the processing and preparation of the sizing agent caused by the inability to evenly disperse SiO2 in the sizing agent; in addition, the polyphenol oxide resin and the epoxy resin covalently linked to SiO2 cooperate with each other, so that the carbon fiber treated with the sizing agent has excellent smooth de-threading performance, reduces the fiber fuzzing of the carbon fiber treated with the sizing agent, and facilitates the subsequent better formation of a composite material between the carbon fiber and the matrix resin.

[0007] In combination with the first aspect, in an optional embodiment of the present application, the polyphenol oxide resin includes at least one of PKHB and PKHH.

[0008] In the above technical scheme, the polyphenol oxide resin is selected from the above substances, which is conducive to further cooperating with the epoxy resin covalently linked to SiO2 to reduce the fiber fuzzing amount of the carbon fiber treated with the sizing agent, and further helps to further improve the interface bonding strength between the carbon fiber treated with the sizing agent and the matrix resin.

[0009] In combination with the first aspect, in an optional embodiment of the present application, the epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and tetrafunctional epoxy resin.

[0010] In the above technical solution, the epoxy resin is selected from the above substances, which is beneficial to further cooperate with the polyphenol oxide resin to reduce the fiber fuzzing amount of the carbon fiber treated with the sizing agent, and further helps to further improve the interface bonding strength between the carbon fiber treated with the sizing agent and the matrix resin.

[0011] In combination with the first aspect, in an optional embodiment of the present application, the emulsifier includes at least one of alkylphenol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyethylene glycol fatty acid ester, polyethylene glycol, sorbitan fatty acid ester and polyoxyethylene sorbitan fatty acid ester.

[0012] In combination with the first aspect, in an optional embodiment of the present application, the mass proportion of the main slurry in the sizing agent is 10-20%.

[0013] In a second aspect, the present application provides a method for preparing a sizing agent provided in any one of the first aspects above, the preparation method comprising: performing a first mixing of a system containing a main slurry and an organic co-solvent to obtain an oily system; then adding water to the oily system and performing a second mixing to obtain an intermediate emulsion; and removing the organic co-solvent in the intermediate emulsion.

[0014] The covalent bonding of SiO2 on the epoxy resin used in the preparation method of the sizing agent provided in the present application can not only significantly increase the surface roughness of the carbon fiber after the sizing agent treatment, but also increase the number of active functional groups on the surface of the carbon fiber after the sizing agent treatment, thereby improving the interfacial bonding strength between the carbon fiber treated with the sizing agent and the matrix resin, and improving the mechanical properties of the composite material formed by the carbon fiber and the matrix resin; compared with directly adding SiO2 to the sizing agent, covalently bonding SiO2 on the epoxy resin is beneficial to avoid the problem of a sharp increase in the viscosity of the sizing agent and difficulty in the processing and preparation of the sizing agent caused by the inability of SiO2 to be evenly dispersed in the sizing agent; in addition, the polyphenol oxide resin used in the preparation method of the sizing agent provided in the present application and the epoxy resin covalently bonded with SiO2 can cooperate with each other, so that the carbon fiber treated with the sizing agent has excellent smooth de-threading performance, reduces the amount of fiber fuzzing of the carbon fiber treated with the sizing agent, and facilitates the subsequent better formation of a composite material between the carbon fiber and the matrix resin.

[0015] In combination with the second aspect, in an optional embodiment of the present application, the organic co-solvent includes at least one of ethanol, acetone, isopropanol, chloroform, dichloromethane, ethyl acetate, methanol, ether and butyl acetate; or / and, the mass proportion of the main slurry in the oily system is 10-15%; or / and, the stirring speed of the second mixing is 5000-8000r / min, and the time of the second mixing is 30-50min.

[0016] In the above technical scheme, the organic co-solvent is selected from the above-mentioned substance, which can more fully dissolve the polyphenol oxide resin and the epoxy resin covalently linked to SiO2, and reduce the viscosity of the oil system, so as to facilitate the subsequent emulsification operation of adding water; the mass proportion of the main slurry in the oil system is 10-15%, which can make the viscosity of the oil system more appropriate, so as to facilitate the subsequent emulsification operation of adding water; the stirring speed of the second mixing is 5000-8000r / min, and the time of the second mixing is 30-50min, so as to facilitate sufficient emulsification to form an emulsion-like sizing agent.

[0017] In combination with the second aspect, in an optional embodiment of the present application, the preparation method of an epoxy resin covalently linked to SiO2 includes: subjecting a silane coupling agent to a first reaction with an ethanol aqueous solution at 50 to 70°C to obtain a hydrolyzate; subjecting the hydrolyzate to a second reaction with SiO2 to obtain SiO2 modified with a silane coupling agent; and subjecting a mixed system containing SiO2 modified with a silane coupling agent, an epoxy resin and ethanol to a third reaction at 50 to 70°C.

[0018] In the above technical solution, an epoxy resin covalently linked to SiO2 can be prepared.

[0019] Optionally, the mass ratio of silane coupling agent to SiO2 is (0.2-0.3):1.

[0020] Optionally, the mass ratio of SiO2 modified by silane coupling agent to epoxy resin is (0.005-0.01):1.

[0021] Optionally, the first reaction time is 20 to 40 minutes.

[0022] Optionally, the second reaction time is 20 to 40 minutes.

[0023] Optionally, the third reaction comprises stirring treatment and ultrasonic treatment performed sequentially, and the time of the stirring treatment and the ultrasonic treatment are each independently 20 to 40 minutes.

[0024] In a third aspect, the present application provides a carbon fiber comprising a carbon fiber matrix and a coating layer located on the surface of the carbon fiber matrix; the coating layer comprises a dried product of a sizing agent as provided in any one of the first aspects above.

[0025] The carbon fiber provided in the present application has a strong interface bonding strength with the matrix resin, which is beneficial to improving the mechanical properties of the composite material formed by the carbon fiber and the matrix resin.

[0026] In a fourth aspect, the present application provides a composite material, which includes a matrix resin and the carbon fiber provided in the third aspect.

[0027] The composite material provided by the present application has good mechanical properties, and the interface bonding strength between the matrix resin and the carbon fiber is high.

[0028] Optionally, the matrix resin comprises a thermoplastic resin.

[0029] Optionally, the thermoplastic resin includes a polyamide resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is a flow chart of the preparation method of the sizing agent provided in this application. DETAILED DESCRIPTION

[0032] The present application provides a sizing agent, which is in the form of an emulsion and includes a main slurry and water; the main slurry includes the following components by weight: 20 to 30 parts of polyphenol oxide resin, 10 to 20 parts of epoxy resin and 10 to 20 parts of emulsifier; wherein SiO2 is covalently bonded to the epoxy resin.

[0033] The present application covalently links SiO2 to the epoxy resin of the sizing agent. After the carbon fiber is treated with the sizing agent, SiO2 can be uniformly loaded on the surface of the carbon fiber, which can not only significantly increase the surface roughness of the carbon fiber after the sizing agent treatment, but also increase the number of active functional groups on the surface of the carbon fiber after the sizing agent treatment, which is beneficial to the physical effect of mechanical engagement between the carbon fiber and the matrix resin, thereby improving the interface bonding strength between the carbon fiber treated with the sizing agent and the matrix resin, and improving the mechanical properties of the composite material formed by the carbon fiber and the matrix resin. Compared with directly adding SiO2 to the sizing agent, covalently linking SiO2 to the epoxy resin is beneficial to avoiding the problem of a sharp increase in the viscosity of the sizing agent and difficulty in the processing and preparation of the sizing agent due to the inability to evenly disperse SiO2 in the sizing agent, and the SiO2 in the sizing agent is evenly dispersed and does not agglomerate.

[0034] In addition, the cooperation between the polyphenol oxide resin and the epoxy resin covalently linked to SiO2 can make the carbon fiber treated with the sizing agent have excellent smooth de-threading performance, and the carbon fiber treated with the sizing agent has a higher smooth de-threading performance, avoiding the problems of sticking and splitting in the de-threading process, and reducing the amount of fiber fuzzing of the carbon fiber treated with the sizing agent, so as to facilitate the subsequent formation of a composite material with the matrix resin.

[0035] As an example, in the main slurry, the weight proportion of the polyphenol oxide resin can be any value among 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts and 30 parts, or a range between any two parts; the weight proportion of the epoxy resin covalently linked to SiO2 can be any value among 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts and 20 parts, or a range between any two parts; the weight proportion of the emulsifier can be any value among 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts and 20 parts, or a range between any two parts.

[0036] In some optional embodiments of the present application, the SiO2 covalently bonded to the epoxy resin is nano-scale silicon dioxide; this is beneficial for further improving the physical effect of mechanical engagement between the carbon fiber and the matrix resin, thereby further improving the interface bonding strength between the carbon fiber treated with the sizing agent and the matrix resin.

[0037] In some optional embodiments of the present application, the polyphenol oxide resin includes at least one of PKHB and PKHH.

[0038] The polyphenol oxide resin uses the above substances, which is beneficial to further cooperate with the epoxy resin covalently linked to SiO2 to reduce the fiber fuzzing amount of the carbon fiber treated with the sizing agent, which is beneficial to further improve the interface bonding strength between the carbon fiber treated with the sizing agent and the matrix resin.

[0039] Furthermore, the polyphenol oxide resin is selected from PKHB.

[0040] In some optional embodiments of the present application, the epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and tetrafunctional epoxy resin.

[0041] The epoxy resin is selected from the above substances, which is beneficial to further cooperate with the polyphenol oxide resin to reduce the fiber fuzzing amount of the carbon fiber treated with the sizing agent, and further helps to further improve the interface bonding strength between the carbon fiber treated with the sizing agent and the matrix resin.

[0042] In some optional embodiments of the present application, the emulsifier includes at least one of alkylphenol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyethylene glycol fatty acid ester, polyethylene glycol, sorbitan fatty acid ester and polyoxyethylene sorbitan fatty acid ester.

[0043] In some optional embodiments of the present application, the mass proportion of the main slurry in the sizing agent is 10-20%.

[0044] As an example, the mass proportion of the main slurry in the sizing agent can be any value among 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% and 20%, or a range between any two values.

[0045] The present application provides a method for preparing a sizing agent, which comprises: first mixing a system containing a main slurry and an organic co-solvent to obtain an oily system; then adding water to the oily system and performing a second mixing to obtain an intermediate emulsion; and removing the organic co-solvent in the intermediate emulsion.

[0046] It should be noted that the selection of components in the main slurry used in the preparation method and the dosage ratio of each component in the sizing agent are the same as the selection of components in the main slurry and the dosage ratio of each component in the sizing agent mentioned above, and will not be repeated here.

[0047] The covalent bonding of SiO2 to the epoxy resin used in the preparation method of the sizing agent provided in the present application can not only significantly increase the surface roughness of the carbon fiber after the sizing agent treatment, but also increase the number of active functional groups on the surface of the carbon fiber after the sizing agent treatment, thereby improving the interfacial bonding strength between the carbon fiber treated with the sizing agent and the matrix resin, and improving the mechanical properties of the composite material formed by the carbon fiber and the matrix resin; compared with directly adding SiO2 to the sizing agent, covalently bonding SiO2 to the epoxy resin is beneficial to avoiding the problem of a sharp increase in the viscosity of the sizing agent and difficulty in the processing and preparation of the sizing agent due to the inability of SiO2 to be evenly dispersed in the sizing agent.

[0048] In addition, the polyphenol oxide resin used in the preparation method of the sizing agent provided in the present application and the epoxy resin covalently linked to SiO2 can cooperate with each other, so that the carbon fiber treated with the sizing agent has excellent smooth de-threading performance, reduces the amount of fiber fuzzing of the carbon fiber treated with the sizing agent, and facilitates the subsequent formation of a composite material with the matrix resin.

[0049] Figure 1 For the flow chart of the preparation method of the sizing agent provided in this application, please refer to Figure 1 , the preparation method of the sizing agent comprises the following steps:

[0050] S110, performing a first mixing of a system containing a main slurry and an organic co-solvent to obtain an oily system; wherein the main slurry comprises the following components by weight: 20 to 30 parts of polyphenol oxide resin, 10 to 20 parts of epoxy resin and 10 to 20 parts of emulsifier; SiO2 is covalently bonded to the epoxy resin.

[0051] In some optional embodiments of the present application, the organic co-solvent includes at least one of ethanol, acetone, isopropanol, chloroform, dichloromethane, ethyl acetate, methanol, ether and butyl acetate.

[0052] The above substances are selected as organic co-solvents, which can more fully dissolve polyphenol oxide resin and epoxy resin covalently linked to SiO2, and reduce the viscosity of the oil system to facilitate the subsequent emulsification operation of adding water.

[0053] In some optional embodiments of the present application, the preparation step of the oily system includes: mixing a polyphenolic resin, an epoxy resin covalently linked to SiO2, and an emulsifier to obtain a main slurry; and then mixing the main slurry with an organic cosolvent to obtain an oily system. Alternatively, the preparation step of the oily system includes: mixing a polyphenolic resin, an epoxy resin covalently linked to SiO2, an emulsifier, and an organic cosolvent to obtain an oily system.

[0054] Furthermore, the mass proportion of the main slurry in the oily system is 10-15%, which can make the viscosity of the oily system more suitable to facilitate the subsequent emulsification operation of adding water.

[0055] As an example, the mass proportion of the main slurry in the oily system can be any value among 10%, 11%, 12%, 13%, 14% and 15%, or a range of values ​​between any two of them.

[0056] In some optional embodiments of the present application, the preparation method of the epoxy resin covalently linked to SiO2 includes: a first reaction of a silane coupling agent and an ethanol aqueous solution at 50-70° C. to obtain a hydrolyzate; a second reaction of the hydrolyzate and SiO2 to obtain SiO2 modified by a silane coupling agent; and a third reaction of a mixed system containing SiO2 modified by a silane coupling agent, an epoxy resin and ethanol at 50-70° C. The above method can prepare an epoxy resin covalently linked to SiO2.

[0057] Illustratively, the temperatures of the first reaction and the third reaction can each independently be any value among 50°C, 52°C, 55°C, 57°C, 60°C, 62°C, 65°C, 67°C and 70°C, or a range between any two of them.

[0058] Furthermore, the mass ratio of the silane coupling agent to SiO2 is (0.2-0.3):1.

[0059] As an example, the silane coupling agent is KH-550, and SiO2 is nano-scale silicon dioxide.

[0060] Furthermore, the mass ratio of SiO2 modified by silane coupling agent to epoxy resin is (0.005-0.01):1.

[0061] Furthermore, the first reaction time is 20 to 40 minutes; the second reaction time is 20 to 40 minutes; the third reaction includes stirring treatment and ultrasonic treatment in sequence, and the stirring treatment and ultrasonic treatment time are each independently 20 to 40 minutes.

[0062] As an example, the time for the first reaction, the second reaction, the stirring treatment and the ultrasonic treatment can each independently be any value among 20min, 22min, 25min, 27min, 30min, 32min, 35min, 37min and 40min, or a range value between any two of them.

[0063] As an example, the second reaction is an ultrasonic dispersion reaction.

[0064] In some optional embodiments of the present application, the preparation method of the above-mentioned hydrolyzate includes: mixing ethanol and water in a mass ratio of (5 to 9): 1, adding hydrochloric acid to adjust the pH to 2 to 4 to obtain an ethanol aqueous solution; and then slowly adding the silane coupling agent dropwise to the aforementioned ethanol aqueous solution and conducting a first reaction at 50 to 70°C.

[0065] Furthermore, the mass ratio of the silane coupling agent to the ethanol aqueous solution is (0.01-0.02):1.

[0066] In some optional embodiments of the present application, the step of the third reaction includes: first ultrasonically dispersing SiO2 modified by a silane coupling agent and ethanol for 20 to 40 minutes to obtain a dispersion; then slowly dropping the aforementioned dispersion into the epoxy resin at 50 to 70°C, and sequentially performing stirring treatment and ultrasonic treatment.

[0067] In some optional embodiments of the present application, the method for preparing an epoxy resin covalently bonded with SiO2 further includes: before performing the third reaction, drying the SiO2 modified with the silane coupling agent in a forced air drying oven (for example, at a temperature of 100°C).

[0068] In some optional embodiments of the present application, the method for preparing an epoxy resin covalently bonded with SiO2 further includes: drying the system after the third reaction in a vacuum oven (for example, at a temperature of 60°C) to remove the ethanol solvent.

[0069] It should be noted that the preparation method of the epoxy resin covalently bonded with SiO2 is not limited to the preparation method provided above, as long as the epoxy resin covalently bonded with SiO2 can be prepared.

[0070] S120, adding water to the oily system and performing a second mixing to obtain an intermediate emulsion.

[0071] Water is added to the oily system and a second mixing is performed to obtain an intermediate emulsion by phase inversion emulsification.

[0072] In some optional embodiments of the present application, water is added to the oily system during stirring of the oily system to facilitate full emulsification.

[0073] In some optional embodiments of the present application, the stirring speed of the second mixing is 5000-8000 r / min, and the time of the second mixing is 30-50 min; so as to fully emulsify and form an emulsion-like sizing agent.

[0074] As an example, the second mixing is homogenous stirring.

[0075] As an example, the water used in the second mixing is deionized water.

[0076] S130, removing the co-solvent in the intermediate emulsion.

[0077] It should be noted that the present application does not limit the specific method for removing the co-solvent, for example, rotary evaporation may be used.

[0078] The present application also provides a carbon fiber, which includes a carbon fiber matrix and a coating layer located on the surface of the carbon fiber matrix; the coating layer includes the dried product of the sizing agent provided above.

[0079] The carbon fiber provided in the present application has a strong interface bonding strength with the matrix resin, which is beneficial to improving the mechanical properties of the composite material formed by the carbon fiber and the matrix resin.

[0080] It should be noted that the present application does not limit the specific material of the carbon fiber matrix.

[0081] The present application also provides a method for preparing carbon fiber, which comprises: coating the above-mentioned sizing agent on the surface of the carbon fiber substrate, and then drying it.

[0082] The present application also provides a composite material, which includes a matrix resin and the carbon fiber provided above.

[0083] The composite material provided by the present application has good mechanical properties, and the interface bonding strength between the matrix resin and the carbon fiber is high.

[0084] In some optional embodiments of the present application, the matrix resin includes a thermoplastic resin.

[0085] As an example, the thermoplastic resin includes a polyamide resin.

[0086] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0087] Example 1

[0088] This embodiment provides a sizing agent and sizing carbon fiber, which are prepared by the following steps:

[0089] (1) Mix ethanol and water in a mass ratio of 9:1, add hydrochloric acid to adjust the pH to 2, and stir evenly to obtain an ethanol aqueous solution; slowly dropwise add silane coupling agent KH-550 into the aforementioned ethanol aqueous solution, reflux and stir at 60° C. for 30 minutes to obtain a hydrolyzate. The mass ratio of silane coupling agent KH-550 to the aforementioned ethanol aqueous solution is 0.01:1.

[0090] The hydrolyzate with a mass ratio of 0.2:1 was mixed with nano-SiO2, dispersed and reacted in an ultrasonic machine for 30 minutes, and then the system after the reaction was dried at 100° C. in a forced air drying oven to obtain SiO2 modified by a silane coupling agent.

[0091] SiO2 modified by silane coupling agent is mixed with ethanol and dispersed by ultrasonic machine for 30 minutes to obtain a dispersion; then the dispersion is slowly added to bisphenol A epoxy resin at 60°C, first magnetically stirred for 30 minutes, then ultrasonically dispersed for 30 minutes, and then transferred to a vacuum oven at 60°C to remove the ethanol solvent to obtain an epoxy resin with covalently linked SiO2. The mass ratio of SiO2 modified by silane coupling agent to bisphenol A epoxy resin is 0.006:1.

[0092] (2) adding phenoxy resin PKHB, epoxy resin covalently linked to SiO2 obtained in step (1) and alkylphenol polyoxyethylene ether in a mass ratio of 25:20:15 into dichloromethane and mixing them evenly to obtain an oily system; then adding deionized water into the oily system and stirring at 6000 r / min for 30 min to obtain an emulsion-like mixed system. Then, volatilizing the dichloromethane in the emulsion-like mixed system to obtain a sizing agent.

[0093] The sum of the masses of the phenoxy resin PKHB, the epoxy resin covalently linked to SiO2, and the alkylphenol polyoxyethylene ether is 10% of the total mass of the oil system; and the mass ratio of the oil system to deionized water is 2:1.

[0094] (3) Using the sizing agent obtained in step (2) to sizing polyacrylonitrile carbon fiber, and then drying to obtain sized carbon fiber.

[0095] Example 2

[0096] The present embodiment provides a sizing agent and sizing carbon fiber. The difference between the present embodiment and the embodiment 1 is that the bisphenol A epoxy resin in step (1) of the embodiment 1 is replaced by bisphenol F epoxy resin, and the mass ratio of SiO2 modified by silane coupling agent to bisphenol F epoxy resin is 0.007:1.

[0097] Example 3

[0098] The present embodiment provides a sizing agent and sizing carbon fiber. The difference between the present embodiment and the embodiment 1 is that the bisphenol A epoxy resin in the step (1) of the embodiment 1 is replaced by a tetrafunctional epoxy resin (purchased from Shanghai Huayi Resin Co., Ltd., model number AG-80), and the mass ratio of SiO2 modified by the silane coupling agent to the tetrafunctional epoxy resin is 0.01:1.

[0099] Comparative Example 1

[0100] This comparative example provides a sizing agent and sizing carbon fiber, which are prepared by the following steps:

[0101] (1) Phenoxy resin PKHB, bisphenol A epoxy resin and alkylphenol polyoxyethylene ether in a mass ratio of 25:20:15 are added to dichloromethane and mixed evenly to obtain an oily system; deionized water is then added to the oily system and stirred at 6000 r / min for 30 minutes to obtain an emulsion-like mixed system. The dichloromethane organic cosolvent in the emulsion-like mixed system is then volatilized to obtain a sizing agent.

[0102] The sum of the masses of phenoxy resin PKHB, bisphenol A epoxy resin and alkylphenol polyoxyethylene ether is 10% of the total mass of the oil system; and the mass ratio of the oil system to deionized water is 2:1.

[0103] (2) Using the sizing agent obtained in step (1) to sizing polyacrylonitrile carbon fiber, and then drying to obtain sized carbon fiber.

[0104] Comparative Example 2

[0105] This comparative example provides a sizing agent and sized carbon fiber. The difference between this comparative example and comparative example 1 is that bisphenol A epoxy resin is replaced by bisphenol F epoxy resin.

[0106] Comparative Example 3

[0107] This comparative example provides a sizing agent and sized carbon fiber. The difference between this comparative example and comparative example 1 is that the bisphenol A epoxy resin is replaced by a tetrafunctional epoxy resin (purchased from Shanghai Huayi Resin Co., Ltd., model AG-80).

[0108] Experimental Example 1

[0109] The sized carbon fibers prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were respectively compounded with PA66 matrix resin to prepare composite materials, and the interlaminar shear strength of the composite materials (according to JC / T 773-2010) was tested. The test results are shown in Table 1.

[0110] Table 1

[0111]

[0112]

[0113] It can be seen from Table 1 that the interlaminar shear strength of the sized carbon fibers prepared in Examples 1 to 3 and the thermoplastic PA66 matrix resin is higher than that of Comparative Examples 1 to 3, indicating that the sized carbon fibers prepared in Examples 1 to 3 and the PA66 matrix resin have a strong interface bonding strength.

[0114] Experimental Example 2

[0115] The fiber fuzzing amounts of the sized carbon fibers after de-spinning obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were compared, and the results are shown in Table 2.

[0116] Table 2

[0117] Fluffing amount (mg / 50m) Example 1 3.2 Example 2 3.7 Example 3 3.5 Comparative Example 1 5.4 Comparative Example 2 6.2 Comparative Example 3 4.9

[0118] It can be seen from Table 2 that the fuzzing amount of the sized carbon fibers prepared in Examples 1 to 3 after de-filamenting is less than that of Comparative Examples 1 to 3, indicating that the sized carbon fibers prepared in Examples 1 to 3 have excellent de-filamenting smoothness performance.

[0119] In summary, the present application covalently links SiO2 to the epoxy resin of the sizing agent, which can not only significantly increase the surface roughness of the carbon fiber treated with the sizing agent, but also increase the number of active functional groups on the surface of the carbon fiber treated with the sizing agent, and reduce the fiber fuzzing amount of the carbon fiber treated with the sizing agent, thereby improving the interface bonding strength between the carbon fiber treated with the sizing agent and the matrix resin, and improving the mechanical properties of the composite material formed by the carbon fiber and the matrix resin.

[0120] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A sizing agent, characterized in that The sizing agent is in the form of an emulsion, and comprises a main slurry and water; the main slurry comprises the following components by weight: 20-30 parts of polyphenol oxide resin, 10-20 parts of epoxy resin and 10-20 parts of emulsifier; Wherein, SiO2 is covalently connected to the epoxy resin.

2. The sizing agent according to claim 1, characterized in that The polyphenol oxide resin includes at least one of PKHB and PKHH.

3. The sizing agent according to claim 1, characterized in that The epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and tetrafunctional epoxy resin.

4. The sizing agent according to claim 1, characterized in that The emulsifier includes at least one of alkylphenol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyethylene glycol fatty acid ester, polyethylene glycol, sorbitan fatty acid ester and polyoxyethylene sorbitan fatty acid ester.

5. The sizing agent according to any one of claims 1 to 4, characterized in that The mass proportion of the main slurry in the sizing agent is 10-20%.

6. A method for preparing a sizing agent according to any one of claims 1 to 5, characterized in that: include: The system containing the main slurry and the organic co-solvent is first mixed to obtain an oily system; then the water is added to the oily system and a second mixing is performed to obtain an intermediate emulsion; and the organic co-solvent in the intermediate emulsion is removed.

7. The method for preparing a sizing agent according to claim 6, characterized in that: The organic co-solvent comprises at least one of ethanol, acetone, isopropanol, chloroform, dichloromethane, ethyl acetate, methanol, ether and butyl acetate; Or / and, the mass proportion of the main slurry in the oily system is 10-15%; Or / and, the stirring speed of the second mixing is 5000-8000 r / min, and the time of the second mixing is 30-50 min.

8. The method for preparing a sizing agent according to claim 6 or 7, characterized in that: The preparation method of the epoxy resin covalently linked to SiO2 comprises: The silane coupling agent and the ethanol aqueous solution are first reacted at 50-70° C. to obtain a hydrolyzate; The hydrolyzate is reacted with SiO2 to obtain SiO2 modified by a silane coupling agent; The mixed system containing SiO2 modified by the silane coupling agent, epoxy resin and ethanol is subjected to a third reaction at 50-70° C.; Optionally, the mass ratio of the silane coupling agent to the SiO2 is (0.2-0.3):1; Optionally, the mass ratio of the SiO2 modified by the silane coupling agent to the epoxy resin is (0.005-0.01):1; Optionally, the first reaction time is 20 to 40 minutes; Optionally, the second reaction time is 20 to 40 minutes; Optionally, the third reaction comprises stirring treatment and ultrasonic treatment performed sequentially, and the time of the stirring treatment and the ultrasonic treatment are each independently 20 to 40 minutes.

9. A carbon fiber, characterized in that: The invention comprises a carbon fiber substrate and a coating layer located on the surface of the carbon fiber substrate; the coating layer comprises the dried product of the sizing agent according to any one of claims 1 to 5.

10. A composite material, characterized in that: comprising a matrix resin and the carbon fiber as claimed in claim 9; Optionally, the matrix resin comprises a thermoplastic resin; Optionally, the thermoplastic resin includes polyamide resin.

Citation Information

Patent Citations

  • High-temperature resistance type nanometer POSS modified epoxy emulsion carbon fiber sizing agent preparation method

    CN105178025A

  • Interface-enhanced nano silicon dioxide-modified epoxy resin sizing agent for carbon fiber

    CN105297448A

  • High-tensile-property carbon fiber composite material

    CN109624430A

  • Method for grafting nanometer silicon dioxide on surface of carbon fiber through ring-opening addition reaction

    CN110512415A

  • Epoxy resin system for energy-absorbing and shock-inhibiting prepreg

    CN116003964A

Cited By

  • Carbon fiber sizing agent for vinyl resin and preparation process of carbon fiber sizing agent

    CN120291360A