Heat-shielding cool fabric and production process thereof

By coating foamed carbon composite material on the fabric and doping zinc oxide, combined with porous silica structure, the problems of insufficient thermal proof performance and UV protection performance of existing thermal proof fabrics are solved, and high thermal insulation and low thermal insulation are achieved Translucent and good cool effect.

CN119061707APending Publication Date: 2024-12-03YIBIN HECHENG TEXTILE TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411184874.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

There is room for improvement in existing heat proof fabrics in terms of heat proofing performance and UV resistance. In particular, PET polyester has weak reflective ability to see light, and the binding force between S iO2, ZnO and lignin is insufficient, resulting in the masking of the fabric. Thermal performance improvement is limited.

Method used

Using foam carbon composite material as the coating of the fabric, by combining zinc oxide and doping N elements, combining porous silica structures to form a coating with low thermal conductivity and high thermal insulation ability, improving the heat shielding of the fabric and UV protection performance, and ensure uniformity and performance of the coating through specific process steps such as stirring, drying, etc.

Benefits of technology

It significantly improves the heat proofing ability and UV resistance of the fabric, reduces the thermal conductivity and light transmittance, enhances the heat insulation and light shading effect of the fabric, and provides a cool feeling, improving the overall performance of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013231810000081
    Figure BDA0005013231810000081
Patent Text Reader

Abstract

The production technology comprises the following steps that deionized water, Tween 80, span 80 and waterborne polyurethane are stirred and mixed in a beaker, foam carbon composite filler is added into the beaker, foam carbon composite filler dispersion liquid is obtained, and the foam carbon composite filler dispersion liquid is added into the beaker; and then uniformly coating the surface of the nylon four-way stretch fabric with the foam carbon composite filler dispersion liquid, and drying the coated fabric in an air dry oven to obtain the heat-shielding cool fabric. According to the prepared heat-shielding cool fabric, the surface of the fabric is coated with the polyurethane coating containing the foam carbon composite material, so that the surface of the fabric is covered with the coating with the low heat conductivity coefficient and the high heat insulation capacity, the fabric has the excellent heat shielding capacity, zinc oxide is compounded in the foam carbon composite material, and the N element is doped in foam carbon, so that the heat-shielding cool fabric is obtained. The ultraviolet absorbing and scattering capabilities of the coating are greatly improved, and the coating has excellent ultraviolet-proof capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fiber reinforced composite materials, relates to functional fiber fabrics, and specifically relates to a heat-shielding and cooling fabric and a production process thereof. Background Art

[0002] With climate change, the daytime temperature in summer is getting higher and higher. People outdoors will be exposed to strong sunlight, which will not only damage the skin with strong ultraviolet rays, but the high temperature generated by continuous exposure will also cause heat stroke, causing great harm to the human body. Therefore, fabrics that can block heat and UV rays are needed to provide protection.

[0003] In the prior art, ultraviolet shielding agents are usually added to fibers, and then the fibers are woven into fabrics, or ultraviolet shielding agents are attached to the surface of fabrics to improve the fabric's anti-ultraviolet ability; by coating the surface of the fabric with a coating or film that can reflect infrared light, the fabric's heat-shielding ability is improved.

[0004] Patent CN117089949A discloses a method for preparing heat-shielding fiber and heat-shielding cooling fabric, using PET polyester as the skin layer and PP polypropylene as the core layer to obtain a heat-shielding fiber with a skin-core structure, which has a good heat-shielding effect; however, PET polyester has a weak reflective ability for visible light and is more dependent on the degree of matting of the matting agent.

[0005] Patent CN117802782A discloses a method for preparing a heat-shielding and UV-proof imitation silk fabric. The fabric has excellent heat-shielding and UV-proof properties by finishing with SiO2 / ZnO / lignin UV shielding agents. The fiber surface is modified with alginate to increase the bonding rate between the UV shielding agent and the fiber. However, this solution is limited by the bonding force between SiO2, ZnO and lignin, and has little effect on improving the heat-shielding performance of the fabric. Summary of the invention

[0006] The object of the present invention is to provide a heat-shielding and cooling fabric and a production process thereof, so as to solve the problem of how to improve the heat-shielding performance of the fabric and provide a cooling feeling and UV protection performance.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A production process of a heat-shielding and cooling fabric comprises the following steps:

[0009] Step 1: Stir and mix the aerogel precursor solution, the expansion material precursor and ethanol in a beaker, add tetraethyl orthosilicate and an ammonia ethanol solution with a concentration of 2 mol / L into the beaker under stirring, heat in an oven at 70-80°C for 24-36h after mixing, and then transfer to a tubular furnace, heat to 500-550°C at a heating rate of 5°C / min under a nitrogen flow of 1L / min, react for 2-3h, cool and grind to nanometer level with a ball mill to obtain a foam carbon composite filler;

[0010] Step 2: Stir deionized water, Tween 80, Span 80 and water-based polyurethane in a beaker, add foam carbon composite filler to the beaker, and stir magnetically for 4-5 hours to obtain a foam carbon composite filler dispersion. Then, evenly apply the foam carbon composite filler dispersion on the surface of the nylon four-way stretch fabric with a coating thickness of 50-80 μm. Dry the coated fabric in a 70-80°C forced air drying oven for 1-2 hours to obtain a heat-shielding and cooling fabric.

[0011] Furthermore, in step 1, the usage ratio of aerogel precursor solution, expansion material precursor, ethanol, tetraethyl orthosilicate and ammonia ethanol solution is 8-10mL:6-8g:10-12mL:10-12mL:0.5-1mL.

[0012] Furthermore, in step 2, the usage ratio of deionized water, Tween 80, Span 80, waterborne polyurethane and foam carbon composite filler is 120-150 mL: 0.15-0.2 g: 0.75-0.85 g: 0.4-0.5 g: 3-4.5 g.

[0013] Further, the expansion material precursor is prepared by the following steps:

[0014] Zn(OH)2, acetic acid, 2-aminoterephthalic acid and DMF are sealed and ground in a stainless steel grinder for 60-90 minutes, assisted by ultrasonic vibration, and then 5-10wt% methanol polyethyleneimine solution is added to the sealing machine, and the sealed grinding is continued for 30-60 minutes, and the expansion material precursor is obtained by filtering, washing and vacuum drying.

[0015] Furthermore, the usage ratio of Zn(OH)2, acetic acid, 2-aminoterephthalic acid, DMF, and 5-10wt% methanol polyethyleneimine solution is 6-8g:1-1.5g:8-10g:5-10mL:5-10g.

[0016] Further, the aerogel precursor solution is prepared by the following steps:

[0017] Methyl orthosilicate and ethanol were stirred and mixed in a beaker to obtain a methyl orthosilicate ethanol dispersion, and an equal volume of the methyl orthosilicate ethanol dispersion was dropped into a sulfuric acid ethanol solution while stirring to obtain an aerogel precursor solution.

[0018] Furthermore, the sulfuric acid ethanol solution is prepared by mixing concentrated sulfuric acid with ethanol, and the mass fraction of the concentrated sulfuric acid in the ethanol is 1-1.5%.

[0019] Furthermore, the usage ratio of methyl orthosilicate and ethanol is 30-40 g:10-15 mL.

[0020] Beneficial effects of the present invention:

[0021] (1) The heat-shielding and cooling fabric prepared by the present invention is coated with a polyurethane coating containing a foam carbon composite material on the surface of the fabric, so that the surface of the fabric is covered with a coating with low thermal conductivity and high thermal insulation capacity, so that the fabric has excellent heat-shielding ability. By compounding zinc oxide in the foam carbon composite material and doping N element in the foam carbon, the ability of the coating to absorb and scatter ultraviolet rays is greatly improved, and the fabric has excellent ultraviolet protection ability.

[0022] (2) The heat-shielding and cooling fabric prepared by the present invention is composited with porous silica and carbon foam structure, which greatly reduces the thermal conductivity of the carbon foam composite material. The carbon foam can block most of the visible light, greatly reducing the light transmittance and improving the thermal insulation capacity of the coating, thereby improving the heat-shielding and light-shielding capabilities of the fabric, improving the heat-shielding effect of the fabric, and making the fabric feel cool through the zinc oxide in the carbon foam. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1: A production process of a heat-shielding and cooling fabric, comprising the following steps:

[0025] Step 1: Grind 6 g Zn(OH)2, 1 g acetic acid, 8 g 2-aminoterephthalic acid and 5 mL DMF in a stainless steel grinder for 60 min, assisted by ultrasonic oscillation at a frequency of 300 Hz, then add 5 g 5 wt% methanol polyethyleneimine solution into the sealed machine, and continue to grind in the stainless steel grinder for 30 min. After filtering out the solid, wash it with DMF and dichloromethane respectively, and then vacuum dry it at 50 ° C for 12 h to obtain an expansion material precursor.

[0026] Step 2: Mix concentrated sulfuric acid and ethanol in a beaker to prepare a 1wt% sulfuric acid ethanol solution, then stir and mix 30g of methyl orthosilicate with 10mL of ethanol to obtain a methyl orthosilicate ethanol dispersion, and add an equal volume of the methyl orthosilicate ethanol dispersion dropwise into the sulfuric acid ethanol solution while stirring to obtain an aerogel precursor solution.

[0027] Step 3: In a beaker, stir and mix 8 mL of aerogel precursor solution, 6 g of expansion material precursor and 10 mL of ethanol, add 10 mL of tetraethyl orthosilicate and 0.5 mL of 2 mol / L ammonia ethanol solution to the beaker under stirring, mix well and heat in an oven at 70 ° C for 24 h, then transfer to a tubular furnace, and heat to 500 ° C at a heating rate of 5 ° C / min under a nitrogen flow of 1 L / min for 2 h. After cooling, grind to nanometer scale using a ball mill to obtain a foam carbon composite filler.

[0028] Step 4: Stir and mix 120 mL of deionized water, 0.15 g of Tween 80, 0.75 g of Span 80 and 0.4 g of aqueous polyurethane in a beaker, add 3 g of foam carbon composite filler to the beaker, stir magnetically for 4 hours to obtain a foam carbon composite filler dispersion, and then evenly apply the foam carbon composite filler dispersion on the surface of the nylon four-way stretch fabric with a coating thickness of 50 μm. Dry the coated fabric in a 70°C forced air drying oven for 1 hour to obtain a heat-shielding and cooling fabric.

[0029] Embodiment 2: A production process of a heat-shielding and cooling fabric, comprising the following steps:

[0030] Step 1: Grind 7 g Zn(OH)2, 1.25 g acetic acid, 9 g 2-aminoterephthalic acid and 7.5 mL DMF in a stainless steel grinder for 75 min, assisted by ultrasonic oscillation at a frequency of 300 Hz, then add 8 g 7 wt% methanol polyethyleneimine solution into the sealed machine, and continue to grind in the stainless steel grinder for 45 min. After filtering out the solid, wash it with DMF and dichloromethane respectively, and then vacuum dry it at 55 ° C for 18 h to obtain an expansion material precursor.

[0031] Step 2: Mix concentrated sulfuric acid and ethanol in a beaker to prepare a 1.25 wt% sulfuric acid ethanol solution, then stir and mix 35 g of methyl orthosilicate with 12.5 mL of ethanol to obtain a methyl orthosilicate ethanol dispersion, and add an equal volume of the methyl orthosilicate ethanol dispersion dropwise to the sulfuric acid ethanol solution while stirring to obtain an aerogel precursor solution.

[0032] Step 3: In a beaker, stir and mix 9 mL of aerogel precursor solution, 7 g of expansion material precursor and 11 mL of ethanol, add 11 mL of tetraethyl orthosilicate and 0.75 mL of 2 mol / L ammonia ethanol solution to the beaker under stirring, mix well and heat at 75 ° C in an oven for 32 h, then transfer to a tubular furnace, and heat to 525 ° C at a heating rate of 5 ° C / min under a nitrogen flow of 1 L / min for 2.5 h. After cooling, grind to nanometer scale using a ball mill to obtain a foam carbon composite filler.

[0033] Step 4: Stir and mix 135 mL of deionized water, 0.17 g of Tween 80, 0.8 g of Span 80 and 0.45 g of aqueous polyurethane in a beaker, add 4 g of foam carbon composite filler to the beaker, stir magnetically for 4.5 hours to obtain a foam carbon composite filler dispersion, and then evenly apply the foam carbon composite filler dispersion on the surface of the nylon four-way stretch fabric with a coating thickness of 70 μm. Dry the coated fabric in a 75°C forced air drying oven for 1.5 hours to obtain a heat-shielding and cooling fabric.

[0034] Embodiment 3: A production process of a heat-shielding and cooling fabric, comprising the following steps:

[0035] Step 1: Grind 8 g Zn(OH)2, 1.5 g acetic acid, 10 g 2-aminoterephthalic acid and 10 mL DMF in a stainless steel grinder for 90 min, assisted by ultrasonic oscillation at a frequency of 300 Hz, then add 10 g 10 wt% methanol polyethyleneimine solution into the sealed machine, and continue to grind in a stainless steel grinder for 60 min. After filtering out the solid, wash it with DMF and dichloromethane respectively, and then vacuum dry it at 60 ° C for 24 h to obtain an expansion material precursor.

[0036] Step 2: Mix concentrated sulfuric acid and ethanol in a beaker to prepare a 1.5 wt% sulfuric acid ethanol solution, then stir and mix 40 g of methyl orthosilicate with 15 mL of ethanol to obtain a methyl orthosilicate ethanol dispersion, and add an equal volume of the methyl orthosilicate ethanol dispersion dropwise to the sulfuric acid ethanol solution while stirring to obtain an aerogel precursor solution.

[0037] Step 3: In a beaker, stir and mix 10 mL of aerogel precursor solution, 8 g of expansion material precursor and 12 mL of ethanol, add 12 mL of tetraethyl orthosilicate and 1 mL of 2 mol / L ammonia ethanol solution to the beaker under stirring, mix well and heat in an oven at 80 ° C for 36 h, then transfer to a tubular furnace, and heat to 550 ° C at a heating rate of 5 ° C / min under a nitrogen flow of 1 L / min for 3 hours. After cooling, grind to nanometer scale using a ball mill to obtain a foam carbon composite filler.

[0038] Step 4: Stir and mix 150 mL of deionized water, 0.2 g of Tween 80, 0.85 g of Span 80 and 0.5 g of aqueous polyurethane in a beaker, add 4.5 g of foam carbon composite filler to the beaker, and stir magnetically for 5 hours to obtain a foam carbon composite filler dispersion. Then, evenly apply the foam carbon composite filler dispersion on the surface of the nylon four-way stretch fabric with a coating thickness of 80 μm. Dry the coated fabric in an 80°C forced air drying oven for 2 hours to obtain a heat-shielding and cooling fabric.

[0039] Principle of the invention:

[0040] The expansion material precursor contains polyethyleneimine, which will decompose at high temperature to produce carbon dioxide, ammonia and water vapor, so that the prepared expansion material has dense pores and expanded volume. The pores can confine static air inside the pores, hindering the thermal convection and heat conduction of the gas, which can reduce the thermal conductivity coefficient and thermal insulation performance of the expansion material and improve the heat shielding performance of the expansion material.

[0041] Silica aerogel can reduce the thermal conductivity coefficient, but the aerogel structure has a high light transmittance. By compounding silica aerogel with carbon, the thermal conductivity coefficient and light transmittance of the composite material can be reduced and the heat shielding effect can be improved.

[0042] During the preparation of silica aerogel, an expansion material precursor is added, and after mixing, the expansion material precursor is expanded and pyrolyzed under nitrogen protection in a tubular furnace. Since the expansion material precursor contains amino groups, pyrolysis can form nitrogen-doped foamed carbon, which can block most of the visible light. At the same time, the high temperature evaporates the solvent of the silica aerogel, so that the generated silica ions are combined with the foamed carbon to form a composite filler with low thermal conductivity and low light transmittance. The Zn atoms in the expansion material precursor are oxidized into zinc oxide in the tubular furnace. The nitrogen-doped carbon and zinc oxide have the ability to absorb and scatter ultraviolet rays, and zinc oxide has a certain cool feeling, which can improve the coolness of the fabric.

[0043] Since the silica surface generated by the aerogel precursor solution is hydrophobic, it affects the dispersibility of the foam carbon composite filler in the aqueous solution. Therefore, Tween 80 and Span 80 are used as emulsifiers to improve the dispersibility of the foam carbon composite filler in the aqueous polyurethane, so that the foam carbon composite filler can be more evenly dispersed on the fabric surface.

[0044] Comparative Example 1: The difference from Example 1 is that no aerogel precursor solution is added in step three.

[0045] Comparative Example 2: The difference from Example 1 is that no expansion material precursor is added in step three.

[0046] Comparative Example 3: The difference from Example 1 is that the preparation method of the foam carbon composite filler is:

[0047] In a beaker, 8 mL of aerogel precursor solution, 6 g of expandable graphite and 10 mL of ethanol were stirred and mixed evenly. Under stirring conditions, 10 mL of tetraethyl orthosilicate and 0.5 mL of 2 mol / L ammonia ethanol solution were added to the beaker. After mixing evenly, the mixture was heated at 70 ° C in an oven for 24 h. Then, the mixture was transferred to a tubular furnace and heated to 500 ° C at a heating rate of 5 ° C / min under a nitrogen flow of 1 L / min for 2 h. After cooling, the mixture was ground to nanometer scale by a ball mill to obtain a foam carbon composite filler.

[0048] The sources of some reagents in the embodiments and comparative examples are as follows:

[0049] Methyl orthosilicate and tetraethyl orthosilicate were purchased from Shanghai MacLean Reagent Co., Ltd.

[0050] Zn(OH)2 was purchased from Jiangsu Pules Biotechnology Co., Ltd.

[0051] Acetic acid, 2-aminoterephthalic acid, DMF, methanol and expandable graphite were purchased from Sigma-Aldrich.

[0052] Tween 80 and Span 80 were purchased from Sinopharm Chemical Reagent Co., Ltd.

[0053] Waterborne polyurethane was purchased from Anhui Anda Huatai New Materials Co., Ltd.

[0054] Polyethylenimine (Mv300) was purchased from West Asia Reagent Co., Ltd.

[0055] The yarn of nylon four-way stretch fabric was purchased from Hangzhou Yinglida Textile Co., Ltd.

[0056] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3. The anti-ultraviolet performance of the heat-shielding and cooling fabric was tested according to GB / T18830-2009, the heat-shielding performance of the heat-shielding and cooling fabric was tested according to GB / T 41560-2022, and the instantaneous coolness coefficient of contact was tested according to GB / T 35263-2017. The results are shown in Table 1:

[0057] Table 1

[0058] It can be seen from Table 1 that the heat-shielding and cooling fabric prepared by the present invention has an excellent ultraviolet protection factor, with a UPF of 594, and a heat-shielding rate of 41.3%. It has good heat-shielding ability and can effectively isolate heat. The instantaneous cool coefficient of contact also reaches 0.22, which is greater than 0.15 in the standard. It is a heat-shielding material with instantaneous cool contact performance, which further improves the comfort and heat-shielding performance of the heat-shielding and cooling fabric.

[0059] In Comparative Example 1, since no aerogel precursor solution is added, nano-silica cannot be well generated, which greatly reduces the silica structure in the foam carbon composite filler. The thermal conductivity of the formed foam carbon composite filler is higher than that of Examples 1 to 3, so the heat shielding rate and ultraviolet protection factor are lower than those of Examples 1 to 3; in Comparative Example 2, since no expansion material precursor is contained, foam carbon cannot be generated, the visible light blocking rate is low, the thermal conductivity is high, and it does not contain zinc oxide, so the ultraviolet protection ability is poor and no cool feeling can be produced; in Comparative Example 3, expandable graphite is used instead of the expansion material precursor. Although a porous carbon structure can be generated and it also has the ability to shield ultraviolet rays, the carbon structure does not contain zinc oxide, and the ultraviolet protection ability is weaker than that of Examples 1 to 3, and the thermal conductivity of the expandable graphite is higher than that of the foam carbon composite filler in Examples 1 to 3, so the heat shielding rate is low.

[0060] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A production process for heat-shielding and cooling fabric, characterized in that: The following steps are involved: Step 1: Stir and mix the aerogel precursor solution, the expansion material precursor and ethanol in a beaker, add tetraethyl orthosilicate and an ammonia ethanol solution with a concentration of 2 mol / L into the beaker under stirring, heat at 70-80°C in an oven for 24-36h after mixing, and then transfer to a tubular furnace, heat to 500-550°C at a heating rate of 5°C / min under a nitrogen flow of 1L / min, react for 2-3h, cool and grind to nanometer level with a ball mill to obtain a foam carbon composite filler; Step 2: Stir deionized water, Tween 80, Span 80 and water-based polyurethane in a beaker, add foam carbon composite filler to the beaker, and stir magnetically for 4-5 hours to obtain a foam carbon composite filler dispersion. Then, evenly apply the foam carbon composite filler dispersion on the surface of the nylon four-way stretch fabric with a coating thickness of 50-80 μm. Dry the coated fabric in a 70-80°C forced air drying oven for 1-2 hours to obtain a heat-shielding and cooling fabric.

2. The production process of a heat-shielding and cooling fabric according to claim 1, characterized in that: The usage ratio of the aerogel precursor solution, the expansion material precursor, ethanol, tetraethyl orthosilicate and the ammonia ethanol solution in step 1 is 8-10 mL: 6-8 g: 10-12 mL: 10-12 mL: 0.5-1 mL.

3. The production process of a heat-shielding and cooling fabric according to claim 1, characterized in that: The usage ratio of deionized water, Tween 80, Span 80, waterborne polyurethane and foam carbon composite filler in step 2 is 120-150 mL: 0.15-0.2 g: 0.75-0.85 g: 0.4-0.5 g: 3-4.5 g.

4. The production process of a heat-shielding and cooling fabric according to claim 1, characterized in that: The expansion material precursor is prepared by the following steps: Zn(OH)2, acetic acid, 2-aminoterephthalic acid and DMF are sealed and ground in a stainless steel grinder for 60-90 minutes, assisted by ultrasonic vibration, and then 5-10wt% methanol polyethyleneimine solution is added to the sealing machine, and the sealed grinding is continued for 30-60 minutes, and the expansion material precursor is obtained by filtering, washing and vacuum drying.

5. The production process of a heat-shielding and cooling fabric according to claim 4, characterized in that: The dosage ratio of the Zn(OH)2, acetic acid, 2-aminoterephthalic acid, DMF and 5-10wt% methanol polyethyleneimine solution is 6-8g:1-1.5g:8-10g:5-10mL:5-10g.

6. The production process of a heat-shielding and cooling fabric according to claim 1, characterized in that: The aerogel precursor solution is prepared by the following steps: Methyl orthosilicate and ethanol were stirred and mixed in a beaker to obtain a methyl orthosilicate ethanol dispersion, and an equal volume of the methyl orthosilicate ethanol dispersion was dropped into a sulfuric acid ethanol solution while stirring to obtain an aerogel precursor solution.

7. The production process of a heat-shielding and cooling fabric according to claim 6, characterized in that: The sulfuric acid ethanol solution is prepared by mixing concentrated sulfuric acid and ethanol, and the mass fraction of the concentrated sulfuric acid in the ethanol is 1-1.5%.

8. The production process of a heat-shielding and cooling fabric according to claim 6, characterized in that: The usage ratio of methyl orthosilicate and ethanol is 30-40 g:10-15 mL.

9. A heat-shielding and cooling fabric, characterized in that: Prepared according to any one of the production processes described in claims 1-8.

Citation Information

Patent Citations

  • Preparation method of heat-shielding fiber and heat-shielding fabric

    CN117089949A

  • Preparation method of heat-shielding and ultraviolet-proof silk-like fabric

    CN117802782A