Method for measuring gas production rate of lithium battery

By using a closed gas path between a buckle battery mold and a pressure detection device in lithium batteries, combined with a U-shaped pressure gauge and an electrical test device, the problems of high equipment cost and low sensitivity in the prior art are solved, and fast and convenient Low-cost, high-sensitivity lithium battery gas production measurement, suitable for large-scale production and new energy industrialization.

CN119063810APending Publication Date: 2024-12-03SHENZHEN DYNANONIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202025.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing lithium battery gas production measurement methods have problems such as high equipment cost, small detection throughput, high detection limit and low sensitivity, which limit their application in large-scale production and rapid testing.

Method used

A closed gas passage is formed by a buckle-type battery mold and a pressure detection device. The gas production volume of the battery is monitored in real time through the pressure detection device. Combined with a U-shaped pressure gauge and an electrical test device, the gas production volume is calculated to achieve fast, convenient, low cost and high sensitivity. measurement.

Benefits of technology

It has realized the measurement of gas production of lithium batteries with low equipment costs, unlimited test throughput and high sensitivity in large-scale industrialization tests. It is suitable for testing conditions in a variety of working conditions, and has promoted the process of industrialization of new energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119063810A_ABST
    Figure CN119063810A_ABST
Patent Text Reader

Abstract

The invention provides a method for measuring the gas production rate of a lithium battery, and belongs to the technical field of lithium battery detection.The method comprises the steps that a positive plate, a negative plate and electrolyte are put into a button cell mold to be assembled to obtain a simulated battery, and a closed gas channel is formed between the button cell mold and a pressure detection device; and the gas production volume of the simulated battery is detected through the pressure detection device. The invention provides a rapid, convenient, low-cost and high-sensitivity method for measuring the gas production of the lithium battery, which has important significance for selecting the optimal synthesis conditions of positive and negative electrode materials, selecting the optimal battery manufacturing parameters and promoting the industrialization process of new energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium battery detection, and in particular relates to a method for measuring gas production of a lithium battery. Background Art

[0002] Lithium batteries have become a key component in new energy technologies due to their high energy density and long service life, especially in electric vehicles and renewable energy storage systems. This type of battery shows obvious advantages over traditional lead-acid batteries and nickel-cadmium batteries. Therefore, the research and development of lithium battery technology has always been a hot topic in scientific research and industry. Although lithium battery technology has made significant progress, there are still many challenges in its materials and manufacturing processes, especially the gas generation problem and related volume expansion problems during battery charging and discharging, which limit the selection and application of certain battery materials.

[0003] At present, the measurement technology of lithium battery gas production is mainly divided into two categories: precision instrument method and drainage / gas method. Precision instrument method includes in-situ differential electrochemical mass spectrometer and volume expansion meter. Differential electrochemical mass spectrometer can monitor and analyze the gas and volatile substances produced in the electrochemical reaction process in real time by combining electrochemical reaction cell and mass spectrometer, and conduct qualitative and quantitative analysis. The volume expansion meter uses multiple high-precision thickness sensors to accurately monitor the expansion of the battery cell during the charging and discharging process, so as to infer the gas production. Although these methods have high detection accuracy, they face the problems of high equipment cost and small test throughput, which limits their application in large-scale production and rapid testing.

[0004] On the other hand, the water displacement method and the gas exhaust method provide lower-cost measurement options. The water displacement method estimates the gas production by measuring the volume of water discharged due to volume expansion caused by gas production in the soft-pack battery cell, while the gas exhaust method calculates the gas production by monitoring the pressure change in a closed system. These methods are simple, low-cost and suitable for rapid detection. However, their main disadvantages include high detection limits, low sensitivity and large error ranges, which are particularly prominent in situations where precise control of production processes and quality assurance are required.

[0005] In summary, although the existing technology provides a variety of methods for measuring the gas production of lithium batteries, each method has its inherent advantages and limitations. The high cost and low throughput of the precision instrument method, as well as the low sensitivity and high error of the drainage / gas method, limit the widespread application of these technologies. These defects highlight the urgent need to develop a new method that is both economical and efficient and can achieve fast and accurate measurements. In addition, for the development of the new energy industry, finding new technical solutions that can overcome these defects is of great industrial and scientific significance. Summary of the invention

[0006] In a first aspect, the present invention provides a method for measuring gas production of a lithium battery, comprising:

[0007] The positive electrode sheet, the negative electrode sheet and the electrolyte are put into a button battery mold to assemble a simulated battery, and a closed gas passage is formed between the button battery mold and a pressure detection device, and the gas production volume of the simulated battery is detected by the pressure detection device.

[0008] In an optional embodiment, the method for measuring the gas production of a lithium battery includes:

[0009] S1, placing the positive electrode sheet and the negative electrode sheet into the sealing detection chamber of the button battery mold respectively;

[0010] S2, drying the assembled button battery mold;

[0011] S3, injecting the electrolyte into the button battery mold after drying to make it soak the positive electrode sheet and the negative electrode sheet;

[0012] S4, connecting the button battery mold to the pressure detection device via the ventilation pipeline, so that a closed gas passage is formed between the sealing detection chamber and the ventilation pipeline and the pressure detection device; and electrically connecting the electrical testing device to the positive electrode sheet and the negative electrode sheet in the sealing detection chamber respectively;

[0013] S5, starting the electrical testing device, running the electrical testing program and recording the testing data of the pressure testing device under different target working conditions;

[0014] S6, calculating the gas production volume of the simulated battery according to the detection data.

[0015] In an optional embodiment, the pressure detection device is a U-shaped pressure gauge;

[0016] Before step S5, the method further includes:

[0017] S7, adjusting the internal liquid level of the U-shaped pressure gauge so that the liquid levels at both ends of the U-shaped tube of the U-shaped pressure gauge are level.

[0018] In an optional embodiment, the liquid in the U-shaped pressure gauge includes any one of water, liquid mercury and silicone oil;

[0019] And / or, step S6 comprises:

[0020] The gas production volume is calculated by the following formula:

[0021] V=πr 2 h;

[0022] Among them, V represents the gas production volume; r represents 1 / 2 of the inner diameter of the U-shaped tube of the U-type pressure gauge; h represents the liquid level height difference of the single-sided U-type pressure gauge.

[0023] In an optional embodiment, any one of the positive electrode sheet, the negative electrode sheet and the electrolyte in the simulated battery is controlled as a variable factor, and the gas production corresponding to the variable factor can be measured.

[0024] In an optional embodiment, the button cell mold is a hollow tubular structure;

[0025] The two ends of the sealing detection chamber of the button battery mold in the length direction are respectively provided with a positive electrode opening and a negative electrode opening;

[0026] The step S1 comprises:

[0027] S11, placing the negative electrode sheet, the separator and the positive electrode sheet into the sealing detection chamber of the button battery mold in sequence through the positive electrode port and / or the negative electrode port;

[0028] S12, covering the positive electrode port and / or the negative electrode port, and respectively contacting the positive electrode sheet and the negative electrode sheet through the conductive medium at the positive electrode port and the negative electrode port.

[0029] In an optional embodiment, the button cell mold is a hollow tubular structure;

[0030] The two ends of the sealing detection chamber of the button battery mold in the length direction are respectively provided with a positive electrode port and a negative electrode port, and a functional port is provided on the button battery mold which is different from the positive electrode port and the negative electrode port;

[0031] The step S3 comprises:

[0032] S31, cooling the button battery mold after drying to room temperature;

[0033] S32, injecting electrolyte from the functional port to seal the functional port;

[0034] S33, leaving the battery at room temperature to allow the electrolyte to soak the positive electrode sheet and the negative electrode sheet in the button battery mold.

[0035] In an optional implementation, the step S4 includes:

[0036] S41, take the ventilation pipeline, connect one end to the functional port, and the other end to the pressure detection device, so that a gas passage is formed between the sealing detection chamber and the pressure detection device;

[0037] S42, electrically connecting the electrical testing device to the conductive medium at the positive electrode port side and the conductive medium at the negative electrode port side in the sealed detection chamber body respectively.

[0038] In an optional embodiment, the drying process comprises at least one of the following conditions:

[0039] A. The drying temperature is not less than 130℃;

[0040] B. Drying time is not less than 2 hours;

[0041] C. The drying process is vacuum drying.

[0042] In an optional implementation manner, before step S1, the method further includes:

[0043] S8, preparing the positive electrode sheet and the negative electrode sheet respectively;

[0044] Preferably, in step S8, the method for preparing the positive electrode sheet includes:

[0045] S81, mixing and slurrying a positive electrode material, a positive electrode binder, a conductive agent and a solvent to obtain a positive electrode slurry;

[0046] S82, coating the positive electrode slurry, and rolling and cutting to obtain a negative electrode positive electrode sheet;

[0047] Preferably, in step S8, the method for preparing the negative electrode sheet includes:

[0048] S83, mixing and slurrying the negative electrode material, the negative electrode binder, the conductive agent and the solvent to obtain a negative electrode slurry;

[0049] S84, coating the negative electrode slurry, and obtaining the negative electrode sheet after rolling and cutting.

[0050] The present invention provides a method for measuring the gas production of a lithium battery, wherein a positive electrode sheet, a negative electrode sheet and an electrolyte are placed in a button battery mold to assemble a simulated battery, and a closed gas passage is formed between the button battery mold and a pressure detection device, and the gas production volume of the simulated battery is detected by the pressure detection device. Compared with precision instrument-based gas measurement methods such as in-situ differential electrochemical mass spectrometers and volume dilatometers, the present invention has low equipment cost, simple assembly, and unlimited test throughput, and is suitable for large-scale industrial testing. Compared with existing water displacement gas measurement methods and exhaust gas measurement methods, the present invention can evaluate the gas production and gas production rate of positive electrode materials in real time and in situ, is reusable, has a low detection limit, and is highly sensitive, and is suitable for trace measurements of small amounts of positive electrode materials, as well as various operating test conditions.

[0051] In summary, the present invention provides a fast, convenient, low-cost, and highly sensitive method for measuring the gas production of lithium batteries, which is of great significance for selecting the optimal synthesis conditions of positive and negative electrode materials, selecting the most suitable battery manufacturing parameters, and promoting the industrialization of new energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 This is a flow chart of a method for measuring gas production of a lithium battery in an embodiment of the present application;

[0053] Figure 2 The overall structure and circuit connection diagram of the detection system based on the lithium battery gas production measurement method in the embodiment of the present application;

[0054] Figure 3 It is a structural schematic diagram of a battery mold of a detection system based on the method for measuring the gas production of a lithium battery in an embodiment of the present application;

[0055] Figure 4 This is a schematic diagram of a formation curve in an embodiment of a method for measuring gas production of a lithium battery of the present application;

[0056] Figure 5 This is a schematic diagram of a rate curve in an embodiment of a method for measuring gas production of a lithium battery in this application.

[0057] Reference numerals:

[0058] 100, detection system; 1, button battery mold; 11, sealed detection chamber; 12, electrode connecting device; 121, positive electrode connecting mechanism; 1211, positive electrode conductive medium; 1212, first connection end; 122, negative electrode connecting mechanism; 1221, negative electrode conductive medium; 1222, second connection end; 13, functional port; 2, ventilation line; 3, electrical testing device; 31, positive terminal; 32, negative terminal; 4, pressure detection device; 200, positive electrode sheet; 300, negative electrode sheet; 400, diaphragm. DETAILED DESCRIPTION

[0059] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] The present application provides a method for measuring the gas production of a lithium battery, comprising:

[0061] The positive electrode sheet, the negative electrode sheet and the electrolyte are put into a button battery mold to assemble a simulated battery, and a closed gas passage is formed between the button battery mold and a pressure detection device, and the gas production volume of the simulated battery is detected by the pressure detection device.

[0062] As mentioned above, the positive electrode sheet, the negative electrode sheet and the electrolyte are placed in the button battery mold to form the "battery" to be tested in this embodiment, that is, the simulated battery.

[0063] The button battery mold is sealed, and the button battery mold is connected to the pressure detection device, thereby forming a closed gas passage between the button battery mold and the pressure detection device.

[0064] The pressure detection device can measure the gas production volume of the electrolyte, the positive electrode sheet and the negative electrode sheet in the button battery mold under different working conditions and different states to generate gas.

[0065] The button battery molds mentioned above may include but are not limited to: standard button battery molds, laboratory button battery molds, Swagelok button battery molds, three-electrode button battery molds, and the like.

[0066] For further reference, Figure 1 , a method for measuring the gas production of lithium batteries, including:

[0067] Step S1, placing the positive electrode sheet and the negative electrode sheet into the sealing detection chamber of the button battery mold respectively.

[0068] As mentioned above, the detection system used in this embodiment refers to Figure 2 , which may include the following structures:

[0069] Button battery mold, ventilation pipeline, electrical test device and pressure detection device.

[0070] The button battery mold is provided with a sealing detection chamber for placing electrolyte, the positive electrode sheet and the negative electrode sheet. The electrical testing device can be electrically connected to the positive electrode sheet and the negative electrode sheet of the battery sample to be tested in the sealing detection chamber. One end of the air guide pipe can be connected to the sealing detection chamber, and the other end can be connected to the pressure detection device.

[0071] As mentioned above, the main parts to be tested in the battery cell whose gas production under different working conditions needs to be tested can be placed in the sealed test cabin, which may include positive electrode sheets and negative electrode sheets, and may also include a diaphragm.

[0072] Step S2, drying the assembled button battery mold.

[0073] The reason for drying the assembled button battery mold is to ensure the dryness and airtightness of the battery assembly, thereby improving the performance and reliability of the battery.

[0074] During the battery manufacturing process, electrodes and other components may absorb a certain amount of moisture. This moisture may cause unpredictable side reactions in the battery's chemical reactions, affecting the battery's performance and life. Drying can effectively remove moisture from components and reduce this risk.

[0075] Drying can also help the airtightness of button battery molds and battery shells, especially for battery types that require high sealing (such as lithium batteries). Good airtightness can prevent the intrusion of external gases and the leakage of internal gases, ensuring the stable operation of the battery.

[0076] In conclusion, the drying process of button battery molds is a critical manufacturing step that can significantly improve the overall performance and safety of the battery, especially in providing a stable electrochemical reaction environment and extending the battery life.

[0077] Step S3, injecting the electrolyte into the button battery mold after drying to make it soak the positive electrode sheet and the negative electrode sheet.

[0078] As mentioned above, injecting electrolyte and ensuring that it fully soaks the battery is a crucial step, because the electrolyte plays a key medium role in the battery, making it possible for ions to transfer between the positive and negative electrodes of the battery.

[0079] The electrolyte is the ion transport medium inside the battery, allowing lithium ions to migrate from the negative electrode to the positive electrode (during discharge) and from the positive electrode to the negative electrode (during charging) during the battery's charge and discharge process. Without the electrolyte, there will be no effective electrochemical reaction inside the battery, and the battery will not work.

[0080] A fully wetted battery can ensure that the contact area between the electrolyte and the electrode material is maximized, which helps to improve the conductivity of lithium ions. If the electrolyte fails to completely wet the electrodes and separators, it will cause a "dead zone" inside the battery where ions cannot be transferred, thereby reducing the overall performance and energy output of the battery.

[0081] Even distribution of electrolyte helps disperse heat evenly during the battery’s charge and discharge process, preventing local overheating and reducing the risk of thermal runaway, a significant concern in battery safety, especially in high-energy-density lithium batteries.

[0082] In short, the injection of electrolyte is to fully wet the pole pieces and diaphragms inside the battery, to ensure the effective migration of lithium ions between the electrodes, thereby ensuring the high performance and response speed of the battery and improving the charging and discharging efficiency of the battery.

[0083] The above steps should be carried out in an oxygen-proof environment (such as a glove box).

[0084] Step S4, connecting the button battery mold to the pressure detection device via the ventilation pipeline, so that a closed gas passage is formed between the sealing detection chamber and the ventilation pipeline and the pressure detection device; and electrically connecting the electrical testing device to the positive electrode sheet and the negative electrode sheet in the sealing detection chamber respectively;

[0085] As mentioned above, the purpose of establishing a sealed gas passage is to monitor the changes in gas pressure generated in real time when the battery is working, so that the gas production during the battery charging and discharging process can be accurately measured, which is an important parameter for evaluating the health status and safety of the battery.

[0086] Step S5, starting the electrical testing device, running the electrical testing program and recording the testing data of the pressure testing device under different target working conditions;

[0087] As described above, the battery charge and discharge test is started by supplying power through the electrical testing device, and the pressure change is recorded to calculate the amount of gas generated, so that the performance of the battery under different charge and discharge conditions can be monitored in real time, which can be used to evaluate the stability and life of the battery.

[0088] Specifically, a battery testing system may be used to charge and discharge the battery, while a data acquisition system may be used to record the readings of the pressure detection device.

[0089] The electrical testing procedures mentioned above may include, but are not limited to: formation, capacity separation, high temperature performance test, low temperature performance test, rate test, cycle test, DC impedance test, etc.

[0090] Step S6, calculating the gas production volume of the simulated battery according to the detection data.

[0091] As described above, the total volume of gas generated by the simulated battery (including the electrolyte, the positive electrode sheet and the negative electrode sheet) is calculated by detecting data using theoretical formulas or empirical formulas, and the obtained gas production data helps evaluate the selection of battery materials and the optimization of battery design.

[0092] The volume of a gas can be calculated using the ideal gas law or a more precise thermodynamic model that takes into account the effects of temperature and pressure.

[0093] This systematic testing method provides an important tool for the development and quality control of lithium batteries, especially in terms of safety and performance evaluation. Through the above steps, we can fully understand the performance of the battery in actual application, so as to make necessary material and design optimization.

[0094] In summary, in the embodiment of the present application, a button battery mold is used, which is connected to the pressure detection device through a ventilation line. During the test, the gas generated in the simulated battery is introduced into the pressure detection device through the ventilation line. The change in air pressure enables the pressure detection device to obtain the corresponding value, measure the change in air pressure, and then calculate the gas production. This method can evaluate the gas production and gas production rate of positive electrode materials in real time and in situ, with a low detection limit, suitable for trace measurement of a small amount of positive electrode materials, and the equipment cost is low, the assembly is simple, and it can be reused, which is suitable for large-scale industrial testing.

[0095] Further, the pressure detection device is a U-shaped pressure gauge;

[0096] Before step S5, the method further includes:

[0097] S7, adjusting the internal liquid level of the U-shaped pressure gauge so that the liquid levels at both ends of the U-shaped tube of the U-shaped pressure gauge are level.

[0098] As mentioned above, the two ends of the U-shaped manometer are connected to different pressure sources. When the pressures at the two ends are different, there will be a height difference in the liquid column in the U-shaped tube. This height difference is caused by the pressure difference. By measuring the height difference of the liquid column, the pressure difference can be calculated because the height difference of the liquid column is directly proportional to the pressure difference.

[0099] U-type pressure gauges are widely used in laboratories and industrial environments, and are particularly suitable for measuring gas pressure differences. It is a common tool for measuring wind speed, wind pressure, furnace pressure, filter pressure drop, etc. It has a wide range of applications in fields such as environmental science, engineering and medical technology. For example, in air conditioning systems and ventilation systems, U-type pressure gauges can help monitor and adjust the pressure level of the system to ensure that the system operates effectively.

[0100] In the gas generation measurement of lithium batteries, the use of a U-type pressure gauge can accurately monitor the internal pressure changes caused by the gas generated by the battery in the working state, thereby evaluating the safety and stability of the battery.

[0101] As mentioned above, the reason for adjusting the liquid levels at both ends of the U-type pressure gauge to the same level before taking pressure measurements is to ensure the accuracy and reliability of the measurement. This adjustment step is to establish an initial reference point so that the subsequent pressure difference can be accurately calculated.

[0102] First, the purpose of adjusting the liquid level to be level is to ensure that there is no pre-existing pressure difference in the U-type manometer before starting the measurement. In this way, any subsequent observed changes in the liquid level can be directly attributed to the pressure changes generated during the test. If the initial liquid level is not balanced, the measured pressure difference will contain an initial error, which will cause the entire measurement result to be inaccurate.

[0103] Secondly, by ensuring that the liquid levels at both ends are level, a clear zero reference is set. This reference point is the basis for all subsequent pressure difference calculations, similar to the need to zero a ruler when taking a length measurement. Any deviation from this reference point clearly indicates the actual pressure change caused by changes in test conditions (such as battery gassing).

[0104] Third, when the liquid levels at both ends of the U-shaped manometer start at the same height, the calculation of the measurement result is simpler and more direct. The pressure difference can be calculated by directly multiplying the liquid level difference by the density of the liquid and the acceleration of gravity, without any adjustment or correction for the initial imbalance.

[0105] Fourth, making this adjustment before starting the experiment also helps reduce errors that may be introduced during operation. For example, changes in ambient temperature or slight movement of the equipment may cause the distribution of the liquid in the tube to change. By ensuring that the liquid levels at both ends are level when starting, you can ensure that these external variables have minimal impact on the final pressure measurement results.

[0106] Finally, in both experimental and industrial applications, it is crucial to standardize the testing process to ensure data consistency and reproducibility. Such adjustments are made by preparing the equipment according to standard operating procedures, ensuring that the setup is the same for each experiment.

[0107] In summary, adjusting the U-type manometer to make the liquid level equal is a key preparation step, which ensures the accuracy and reliability of the measurement and provides the necessary conditions for accurate measurement of pressure difference. This not only helps to improve the accuracy of the data, but also helps to analyze and evaluate the performance of the battery or other system under controlled conditions.

[0108] Furthermore, the liquid in the U-shaped pressure gauge includes any one of water, liquid mercury and silicone oil.

[0109] It should be noted that when the electrode diameter is small and the gas production is small, it is necessary to choose high-density liquid mercury as the built-in liquid to help improve the detection limit.

[0110] When the electrodes need to avoid water, choosing silicone oil as the built-in liquid is beneficial to maintaining the sealing and dryness of the system.

[0111] By selecting different liquids in the U-shaped pressure gauge, it can flexibly adapt to the detection needs of different battery poles.

[0112] Furthermore, the step S6 comprises:

[0113] The gas production volume is calculated by the following formula:

[0114] V=πr 2 h;

[0115] Among them, V represents the gas production volume; r represents 1 / 2 of the inner diameter of the U-shaped tube of the U-type pressure gauge; h represents the liquid level height difference of the single-sided U-type pressure gauge.

[0116] This formula is used to calculate the volume of a cylinder due to the change in gas volume caused by a pressure difference. In the application of U-type manometers, this formula helps to convert the liquid level difference into the corresponding gas volume, thereby quantifying the amount of gas generated by the battery.

[0117] V: represents the gas production volume, usually in cubic meters (m 3 ) or cubic centimeters (cm 3 ).

[0118] π (pi): A mathematical constant approximately equal to 3.14159, used in circular geometry calculations.

[0119] r: represents the radius of the U-shaped tube of the U-type pressure gauge, which is half of the inner diameter. Determining this value is critical because it directly affects the accuracy of the volume calculation.

[0120] h: represents the liquid level difference of a single-sided U-shaped pressure gauge. This is the height difference between the height of mercury or other liquid rising or falling on one side of the U-shaped tube and the height difference on the other side caused by the pressure difference.

[0121] The formula essentially calculates the volume of a cylinder. The cylinder here represents the space created by the column of liquid moving in the U-shaped manometer due to the pressure change, which can be thought of as the volume of gas corresponding to the pressure difference. This calculation assumes that under the action of pressure, the space created by the movement of liquid in the U-shaped tube is equal to the volume of gas produced.

[0122] In actual operation, the liquid level on one side of the U-shaped manometer will drop due to the increase in gas pressure, while the liquid level on the other side will rise accordingly. This height difference h is directly measured. The inner diameter (or radius r) of the U-shaped manometer must be measured accurately, because the accuracy of the volume calculation is directly affected by its accuracy. Usually, this inner diameter is determined when the manometer is manufactured and marked on the device.

[0123] In lithium battery testing, gases may be generated or consumed when the battery is charged or discharged. These changes cause pressure changes in the manometer, which in turn causes changes in the height of the liquid level. By measuring this height difference and using the above formula, the total volume of gas generated or consumed by the electrochemical reaction can be accurately calculated, which is crucial for evaluating the safety and performance of the battery.

[0124] By understanding and applying this formula, researchers and engineers can better monitor and analyze the behavior of batteries during operation, especially as it relates to the gas dynamics inside the battery. This analysis is valuable for optimizing battery design and enhancing battery safety.

[0125] Furthermore, any one of the positive electrode sheet, the negative electrode sheet and the electrolyte in the simulated battery is controlled as a variable factor, and the gas production corresponding to the variable factor can be measured.

[0126] As mentioned above, the measurement method provided in the embodiments of the present application has certain flexibility and variability. Specifically, when measuring the gas production of a lithium battery, the influence of this variable factor on the gas production of the lithium battery can be measured separately by changing one of the three key components in the simulated battery, namely, the positive electrode, the negative electrode or the electrolyte.

[0127] It can be seen that the embodiments of the present application provide an experimental design idea, which allows researchers or technicians to study how this variable affects the gas production of lithium batteries under specific conditions by controlling a variable in the experiment (positive electrode, negative electrode or electrolyte). This method helps to more accurately understand the specific effects of different materials or conditions on battery performance, thereby providing a scientific basis for battery design and material selection.

[0128] For example, if you want to evaluate the effect of different cathode materials on the gas production of lithium batteries, you can keep the anode and electrolyte unchanged in the experiment and only change the type or composition of the cathode. By comparing the gas production under different cathode configurations, you can determine which cathode material performs better in gas production. The same method can also be applied to the evaluation of anode and electrolyte.

[0129] In a preferred embodiment, the button battery mold is a button battery mold with a hollow tubular structure;

[0130] The two ends of the sealing detection chamber of the button battery mold in the length direction are respectively provided with a positive electrode opening and a negative electrode opening;

[0131] As mentioned above, the button battery mold can be a hollow tubular structure, and its cross section can be circular, rectangular, or other shapes.

[0132] The step S1 comprises:

[0133] Step S11, placing the negative electrode sheet, the separator and the positive electrode sheet into the sealing detection chamber of the button battery mold in sequence through the positive electrode port and / or the negative electrode port;

[0134] Step S12, covering the positive electrode port and / or the negative electrode port, and respectively contacting the positive electrode sheet and the negative electrode sheet through the conductive medium at the positive electrode port and the negative electrode port.

[0135] Above, in the detection system, reference Figure 3 , the button battery mold may also include an electrode connecting device;

[0136] The electrode connecting device is detachably connected to the sealing detection chamber body;

[0137] Furthermore, the electrode connection device can electrically connect the positive electrode sheet and the negative electrode sheet of the battery sample to be tested to the corresponding positive terminal and negative terminal of the electrical testing device respectively.

[0138] The electrode connection device includes a positive electrode connection mechanism and a negative electrode connection mechanism;

[0139] One end of the positive electrode connection mechanism is electrically connected to the positive electrode sheet of the battery sample to be tested, and the other end is connected to the positive terminal of the electrical testing device;

[0140] One end of the negative electrode connection mechanism is electrically connected to the negative electrode sheet of the battery sample to be tested, and the other end is connected to the negative terminal of the electrical testing device.

[0141] The positive electrode connection mechanism includes a positive electrode conductive medium and a first connection end connected to the positive electrode conductive medium;

[0142] The negative electrode connection mechanism includes a negative electrode conductive medium and a second connection end connected to the negative electrode conductive medium;

[0143] The positive electrode conductive medium and the negative electrode conductive medium can be placed in the sealed detection chamber, and respectively abut against and electrically connect with the positive electrode sheet and the negative electrode sheet of the battery sample to be tested;

[0144] The first connection end is used to connect to the positive terminal of the electrical testing device;

[0145] The second connection end is used to be connected to the negative terminal of the electrical testing device.

[0146] As mentioned above, after the positive electrode sheet and the negative electrode sheet are placed in the sealed detection chamber, electrode connecting devices are respectively provided at both ends, and the corresponding positive electrode connecting mechanism and negative electrode connecting mechanism can be used to abut with a certain force, so that the positive electrode sheet, the diaphragm and the negative electrode sheet are squeezed by external force, so that the positive electrode sheet and the negative electrode sheet can be electrically connected to the electrical testing device respectively.

[0147] As mentioned above, the conductive medium may be a stainless steel electrode or a glassy carbon electrode, or may be a conductive testing device made of other materials.

[0148] The above structure is the preparatory stage for setting up the positive electrode sheet and the negative electrode sheet to form a simulated battery, wherein the positive electrode sheet and the negative electrode sheet of the simulated battery are physically connected through corresponding conductive media (such as conductive glue or metal contacts) to ensure that the current can flow smoothly during the charging and discharging process, thereby establishing a stable electrical connection and providing a basis for the subsequent battery test.

[0149] In a preferred embodiment, the button battery mold is a button battery mold with a hollow tubular structure;

[0150] The two ends of the sealing detection chamber of the button battery mold in the length direction are respectively provided with a positive electrode port and a negative electrode port, and a functional port is provided on the button battery mold which is different from the positive electrode port and the negative electrode port;

[0151] As mentioned above, the functional port can be set in the middle position of the battery mold or in other positions. In addition, the functional port can be provided with a plug to play a certain sealing role before and after the injection of electrolyte or other treatments.

[0152] The step S3 comprises:

[0153] S31, cooling the button battery mold after drying to room temperature;

[0154] S32, injecting electrolyte from the functional port to seal the functional port;

[0155] S33, leaving the battery at room temperature to allow the electrolyte to soak the positive electrode sheet and the negative electrode sheet in the button battery mold.

[0156] The functional port can be used as an electrolyte injection port and a port for connecting to a ventilation line for gas production detection. In addition, different ports can be set according to the specific structure and function.

[0157] Furthermore, the step S4 includes:

[0158] S41, take the ventilation pipeline, connect one end to the functional port, and the other end to the pressure detection device, so that a gas passage is formed between the sealing detection chamber and the pressure detection device;

[0159] S42, electrically connecting the electrical testing device to the conductive medium at the positive electrode port side and the conductive medium at the negative electrode port side in the sealed detection chamber body respectively.

[0160] As mentioned above, the gas line connection can be operated in a glove box.

[0161] The ventilation pipeline can be a silicone rubber hose.

[0162] For example, the sealing bolts of the battery mold can be first removed, and a silicone rubber hose with matching size can be placed on the liquid injection port. A fixed amount of liquid is built into the U-shaped pressure gauge, and a silicone rubber hose is placed on one end of the U-shaped pressure gauge.

[0163] The silicone rubber hose is connected via a reducing straight pipe joint to form a gas passage between the battery mold and the U-type pressure gauge.

[0164] In a preferred embodiment, sealing materials may be used for winding and sealing, or for covering and sealing at the connection between the ventilation line and the pressure detection device, and at the connection between the ventilation line and the sealing detection chamber.

[0165] As mentioned above, the interfaces in the embodiments of the present application are all sealed by wrapping polytetrafluoroethylene tape to prevent air leakage, and the liquid column in the U-shaped pressure gauge also acts as a liquid seal.

[0166] Furthermore, the drying process comprises at least one of the following conditions:

[0167] A. The drying temperature is not less than 130℃;

[0168] B. Drying time is not less than 2 hours;

[0169] C. The drying process is vacuum drying.

[0170] The drying time is not less than 2 hours of vacuum drying, which can further improve the drying efficiency.

[0171] Furthermore, before step S1, the method further includes:

[0172] Step S8, preparing the positive electrode sheet and the negative electrode sheet respectively;

[0173] Furthermore, in step S8, the method for preparing the positive electrode sheet includes:

[0174] S81, mixing and slurrying a positive electrode material, a positive electrode binder, a conductive agent and a solvent to obtain a positive electrode slurry;

[0175] S82, coating the positive electrode slurry, and rolling and cutting to obtain a negative electrode positive electrode sheet;

[0176] Wherein, the positive electrode sheet may be a circular electrode sheet after cutting;

[0177] For example, the positive electrode material is mixed with the positive electrode binder, conductive agent, and solvent to make a slurry, and then coated on one side of the aluminum foil to make a positive electrode sheet. The surface of the electrode sheet should be smooth and free of obvious cracks and faults. The electrode sheet is rolled under a certain pressure and then placed on a sheet punching machine. Among them, it can be cut into a circular positive electrode sheet.

[0178] As mentioned above, the positive electrode material may be lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide, etc., with a content of 80%-95%;

[0179] As mentioned above, the positive electrode binder may be polyvinylidene fluoride, polymethyl methacrylate, etc., with a content of 2.0%-4.0%;

[0180] As mentioned above, the conductive agent may be Ketjen black, carbon fiber, carbon nanotube, graphene, etc., with a content of 0.5%-3.5%;

[0181] As mentioned above, the solvent may be N-methylpyrrolidone, dimethyl sulfoxide, dimethylformamide, etc., and the added amount is 50%-60% of the content of lithium manganese iron phosphate.

[0182] As mentioned above, the rolling pressure of the electrode sheet is 8-200T, and the diameter of the circular positive electrode sheet is 10-40mm.

[0183] Furthermore, in step S8, the method for preparing the negative electrode sheet includes:

[0184] S83, mixing and slurrying the negative electrode material, the negative electrode binder, the conductive agent and the solvent to obtain a negative electrode slurry;

[0185] S84, coating the negative electrode slurry, and obtaining the negative electrode sheet after rolling and cutting.

[0186] Wherein, the negative electrode sheet may be a circular electrode sheet after cutting.

[0187] For example, the negative electrode material is mixed with the negative electrode binder, conductive agent, and solvent to make a slurry, and then coated on one side of the copper foil to make a negative electrode sheet. The surface of the electrode sheet should be smooth and free of obvious cracks and faults. The electrode sheet is rolled under a certain pressure and then placed on a punching machine. It can be cut into a circular negative electrode sheet.

[0188] In addition, metal lithium sheets can also be directly used as negative electrode sheets.

[0189] As mentioned above, the negative electrode material can be graphite carbon, lithium titanate, silicon carbon negative electrode, etc., with a content of 90%-97%;

[0190] As mentioned above, the negative-stage binder may be styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, polyacrylonitrile, polyacrylate, etc., with a content of 0.5%-5%;

[0191] As mentioned above, the conductive agent may be carbon black, carbon fiber, carbon nanotube, graphene, etc., with a content of 0.5%-4%;

[0192] As mentioned above, the solvent may be deionized water or other chemical reagent aqueous solution, and the added amount is 85%-95% of the content of the conductive graphite. The negative electrode may also directly use a metal lithium sheet.

[0193] The separator mentioned above may be a circular Celgard 2400 microporous polypropylene membrane with a diameter of 12 to 42 mm.

[0194] The present invention is further described below by means of specific examples, but it should be understood that these examples are only used for more detailed description and should not be construed as limiting the present invention in any form.

[0195] Embodiment 1:

[0196] In this embodiment, the following method was used to detect the gas production during the formation of lithium manganese iron phosphate-graphite button-type full cells.

[0197] Experimental methods:

[0198] (1) 9 g of polyvinylidene fluoride, 5 g of Ketjen black, and 300 g of N-methylpyrrolidone were mixed into a conductive slurry, and 200 g of lithium iron manganese phosphate was added to prepare a positive electrode sheet, which was rolled at a pressure of 25 T.

[0199] (2) 13 g of styrene-butadiene rubber, 3.2 g of carboxymethyl cellulose, 12.8 g of Ketjen black, and 266 g of deionized water were mixed into a conductive slurry, and 300 g of graphite carbon was added to prepare a negative electrode sheet, which was then rolled at a pressure of 25 T.

[0200] (3) Place a 28 mm diameter positive electrode sheet, a 32 mm diameter separator, and a 30 mm diameter negative electrode sheet into a button cell mold.

[0201] (4) The button cell mold was baked at 130°C for 3 h, transferred to a glove box, injected with 1 mL of electrolyte, tightened the sealing bolts, and left at room temperature for 3 h.

[0202] (5) After connecting the gas line, add silicone oil to the U-shaped tube, start the formation process, and record the value and height of the U-shaped pressure gauge under different voltage changes.

[0203] Embodiment 2:

[0204] In this embodiment, the gas production during the formation of lithium manganese iron phosphate-graphite button-type full cells was detected.

[0205] Experimental methods:

[0206] It is basically the same as Example 1, and the difference from Example 1 is that:

[0207] (1) Place a 14 mm diameter positive electrode sheet, an 18 mm diameter separator, and a 16.5 mm diameter negative electrode sheet into a button cell mold.

[0208] (2) The button cell mold was baked at 130°C for 3 h, transferred to a glove box, injected with 0.25 mL of electrolyte, tightened the sealing bolts, and left at room temperature for 3 h.

[0209] (3) After connecting the gas line, add liquid mercury to the U-shaped tube, start the formation step, and record the value and height of the U-shaped pressure gauge under different voltage changes.

[0210] Embodiment 3:

[0211] In this embodiment, the gas production of lithium manganese iron phosphate-graphite button-type full battery was detected.

[0212] Experimental methods:

[0213] It is basically the same as Example 1, and the difference from Example 1 is that:

[0214] (1) After the gas line is connected, start the multiplication step and record the value and height of the U-type pressure gauge at different stages.

[0215] Comparative Example 1:

[0216] In this comparative example, the gas production of lithium iron manganese phosphate-graphite monolithic soft-pack battery was detected.

[0217] Experimental methods:

[0218] (1) Cut the positive electrode sheet rolled by single-sided coating into a rectangle with a width of 43 mm and a length of 56 mm, scrape powder at the upper right corner, weld the aluminum tab with a width of 6 mm and a length of 7 mm, and apply the tab glue.

[0219] (2) Cut the negative electrode sheet pressed by the double-sided coating roller into a rectangle with a width of 44 mm and a length of 58 mm, scrape powder at the upper right corner, weld the nickel tab, the tab width is 6 mm and the length is 7 mm, and stick the tab glue.

[0220] (3) The diaphragm is 60 mm wide and 250 mm long.

[0221] (4) Making a battery cell: Place a single-sided positive electrode sheet on the diaphragm and fix it with a spring clip, then cover the diaphragm on the positive electrode sheet. Similarly, place a double-sided negative electrode sheet, cover it with a diaphragm, place another single-sided positive electrode sheet, and cover it with a diaphragm. After stacking the sheets, use scissors to cut off the excess diaphragm at the bottom positive electrode sheet, and then wrap the top diaphragm around the core one and a half times. Finally, use high-temperature glue to fix the battery cell and the tabs.

[0222] (5) Making a battery pack: Use a cutting machine to cut the aluminum-plastic film into a rectangle of 150 mm × 130 mm, then fold the 150 mm long side in half, and then use a side sealing machine to heat-seal the two top corners of the folded aluminum-plastic film. Place the battery cell in the aluminum-plastic film bag, with the positive electrode ear glue exposed on the left side and the negative electrode ear glue exposed on the right side.

[0223] (6) Sealing and baking: Use a sealing machine, set the temperature to 180°C, and set the time to 4s. Send the top edge of the battery under the heat seal bar for top sealing, so that the two layers of aluminum-plastic film and the positive and negative tabs fit together. Send the side edge of the battery under the heat seal bar for side sealing, so that the two layers of aluminum-plastic film fit together. Place the battery pack in a vacuum oven at -90Kpa and 85°C and bake for 16 hours.

[0224] (7) Liquid injection: The baked battery pack is transferred to a glove box, 1 mL of electrolyte is injected, and the pack is sealed using a vacuum sealer at a temperature of 170°C. After liquid injection and sealing, the single-piece soft-pack battery is placed at 45°C and normal pressure for 3 to 4 hours.

[0225] (8) Place a beaker filled with 1L of water on a balance, remove the tares, put in a single soft-pack battery, and record the weight as m1. Take out the battery pack, wipe it dry, and connect the tabs to the electrical test fixture.

[0226] (9) Start the formation process: charge at 0.05C for 2.4 hours, charge at 0.2C for 2 hours, and charge at 0.2C for 20 minutes.

[0227] (10) Place the expanded single-piece soft-pack battery into the beaker in step (8), ensuring that the battery pack is at the same liquid level twice, and record the weight as m2.

[0228] (11) Gas production volume V = (m1-m2) / ρ 水 .

[0229] Experimental results and analysis:

[0230] 1. Formation curves for Example 1 and Example 2:

[0231] refer to Figure 4 , are the formation curves of Examples 1 and 2. The difference between the two is the electrode area. The electrode area of ​​Example 1 is four times that of Example 2. The formation steps remain consistent. The capacity of Example 2 is smaller than that of Example 1.

[0232] 2. Rate curve for Example 3:

[0233] refer to Figure 5 , is the rate curve of lithium manganese iron phosphate. As the discharge rate increases, the discharge capacity gradually decreases. When discharged at a rate of 3C, the capacity retention rate remains at 99.81%. These results show that the battery mold will not affect its performance when connected to the gas path.

[0234] 3. Gas production data:

[0235] (1) Embodiment 1:

[0236] Table 1. Gas production data test results of Example 1

[0237]

[0238] Table 1 shows the gas production data at each voltage stage of Example 1.

[0239] According to the data in Table 1, the gas production is the largest and the gas production rate is the fastest at the initial stage of voltage rise; in the low current charging stage, the battery gas production is much higher than that in the high current charging stage.

[0240] (2) Embodiment 2:

[0241] Table 2. Gas production data test results of Example 2

[0242]

[0243] Table 2 is the gas production data of Example 2 at each voltage stage. The difference between Example 2 and Example 1 is the area of ​​the electrode, which accounts for 25% of the area of ​​Example 1. According to the data in Table 2, it is consistent with the gas production law in Example 1, and the gas production is close to 25% of that in Example 1. It can be seen that the battery gas production is positively correlated with the cell area.

[0244] (3) Embodiment 3:

[0245] Table 3. Gas production data test results of Example 3

[0246] Constant power step Voltage changes Gas production / mL Let stand for 3 hours 2.9985-2.9982 0.000 0.5C constant current and constant voltage charging 2.9982-4.25 0.172 0.2C discharge 4.25-2.00 0.015 0.5C constant current and constant voltage charging 2.00-4.25 0.033 0.5C discharge 4.25-2.00 0.009 0.5C constant current and constant voltage charging 2.00-4.25 0.019 1C discharge 4.25-2.00 0.005 0.5C constant current and constant voltage charging 2.00-4.25 0.000 2C discharge 4.25-2.00 0.000 0.5C constant current and constant voltage charging 2.00-4.25 0.000 3C discharge 4.25-2.00 0.000 Summary 0.253

[0247] Table 3 shows the gas production values ​​at each stage when lithium manganese iron phosphate is charged at 0.5C and discharged at 0.2, 0.5, 1, 2, and 3C. In the initial 0.5C charging stage, the corresponding gas production value is close to that in Example 1. In the 0.2C discharge stage, a small amount of gas is generated. In the second round of 0.5C charging stage, a small amount of gas will be generated again, but the amount of gas is much less than the first charge. When discharging at different rates subsequently, the gas generation gradually decreases until the discharge rate reaches 2C and the gas production stops.

[0248] (4) Comparative Example 1:

[0249] Table 4. Gas production data test results of Comparative Example 1

[0250] Battery ID <![CDATA[m1(g)]]> <![CDATA[m2(g)]]> <![CDATA[ΔV(cm 3 )]]> 1 11.34 11.44 0.10 2 11.32 12.35 1.03 3 13.15 12.63 -0.52

[0251] Table 4 shows the gas production data of the single-chip soft-pack battery made from the same batch of materials in Example 1. The three measurement results differ greatly, proving that there is a large error in measuring the gas production using the water displacement method. In addition, the area of ​​the pole piece used in Example 1 is 31 times that of the pole piece used in Example 2, indicating that the water displacement method has a low detection limit and is not suitable for hard-shell batteries, and cannot measure the gas production under various test conditions in real time.

[0252] In summary, the method provided in this application can stably identify a small amount of gas and measure the gas production under various voltage changes in real time without affecting the normal performance of the battery. The test results show that the gas production is positively correlated with the area of ​​the positive electrode, and the initial charging stage is the peak period of gas production, which is speculated to be related to the formation of the SEI film. Compared with the drainage method, this method can accurately test the gas production, identify a small amount of gas production, with relatively small errors, and is simple to operate and highly accurate.

[0253] The above are preferred implementation modes and corresponding embodiments of the present invention. It should be pointed out that, for those skilled in the art, without departing from the creative concept of the present invention, several modifications and improvements may be made, including but not limited to the adjustment of proportions, processes, dosages and reaction vessels, which all fall within the scope of protection of the present invention.

Claims

1. A method for measuring gas production of a lithium battery, characterized in that: include: The positive electrode sheet, the negative electrode sheet and the electrolyte are put into a button battery mold to assemble a simulated battery, and a closed gas passage is formed between the button battery mold and a pressure detection device, and the gas production volume of the simulated battery is detected by the pressure detection device.

2. The method for measuring gas production of a lithium battery according to claim 1, characterized in that: The method for measuring the gas production of a lithium battery comprises: S1, placing the positive electrode sheet and the negative electrode sheet into the sealing detection chamber of the button battery mold respectively; S2, drying the assembled button battery mold; S3, injecting the electrolyte into the button battery mold after drying to make it soak the positive electrode sheet and the negative electrode sheet; S4, connecting the button battery mold to the pressure detection device via the ventilation pipeline, so that a closed gas passage is formed between the sealing detection chamber and the ventilation pipeline and the pressure detection device; and electrically connecting the electrical testing device to the positive electrode sheet and the negative electrode sheet in the sealing detection chamber respectively; S5, starting the electrical testing device, running the electrical testing program and recording the testing data of the pressure testing device under different target working conditions; S6, calculating the gas production volume of the simulated battery according to the detection data.

3. The method for measuring gas production of a lithium battery as claimed in claim 2, characterized in that: The pressure detection device is a U-shaped pressure gauge; Before step S5, the method further includes: S7, adjusting the internal liquid level of the U-shaped pressure gauge so that the liquid levels at both ends of the U-shaped tube of the U-shaped pressure gauge are level.

4. The method for measuring gas production of a lithium battery as claimed in claim 3, characterized in that: The liquid in the U-type pressure gauge includes any one of water, liquid mercury and silicone oil; And / or, step S6 comprises: The gas production volume is calculated by the following formula: V=πr 2 h; Among them, V represents the gas production volume; r represents 1 / 2 of the inner diameter of the U-shaped tube of the U-type pressure gauge; h represents the liquid level height difference of the single-sided U-type pressure gauge.

5. The method for measuring gas production of a lithium battery according to claim 1, wherein: Any one of the positive electrode sheet, the negative electrode sheet and the electrolyte in the simulated battery is controlled as a variable factor, and the gas production corresponding to the variable factor can be measured.

6. The method for measuring gas production of a lithium battery as claimed in claim 2, characterized in that: The button battery mold is a hollow tubular structure; The two ends of the sealing detection chamber of the button battery mold in the length direction are respectively provided with a positive electrode opening and a negative electrode opening; The step S1 comprises: S11, placing the negative electrode sheet, the separator and the positive electrode sheet into the sealing detection chamber of the button battery mold in sequence through the positive electrode port and / or the negative electrode port; S12, covering the positive electrode port and / or the negative electrode port, and respectively contacting the positive electrode sheet and the negative electrode sheet through the conductive medium at the positive electrode port and the negative electrode port.

7. The method for measuring gas production of a lithium battery as claimed in claim 2, characterized in that: The button battery mold is a hollow tubular structure; The two ends of the sealing detection chamber of the button battery mold in the length direction are respectively provided with a positive electrode port and a negative electrode port, and a functional port is provided on the button battery mold which is different from the positive electrode port and the negative electrode port; The step S3 comprises: S31, cooling the button battery mold after drying to room temperature; S32, injecting electrolyte from the functional port to seal the functional port; S33, leaving the battery at room temperature to allow the electrolyte to soak the positive electrode sheet and the negative electrode sheet in the button battery mold.

8. The method for measuring gas production of a lithium battery as claimed in claim 7, characterized in that: The step S4 comprises: S41, take the ventilation pipeline, connect one end to the functional port, and the other end to the pressure detection device, so that a gas passage is formed between the sealing detection chamber and the pressure detection device; S42, electrically connecting the electrical testing device to the conductive medium at the positive electrode port side and the conductive medium at the negative electrode port side in the sealed detection chamber body respectively.

9. The method for measuring gas production of a lithium battery as claimed in claim 2, characterized in that: The drying process conditions include at least one of the following conditions: A. The drying temperature is not less than 130℃; B. Drying time is not less than 2 hours; C. The drying process is vacuum drying.

10. The method for measuring gas production of a lithium battery as claimed in claim 2, characterized in that: Before step S1, the method further includes: S8, preparing the positive electrode sheet and the negative electrode sheet respectively; Preferably, in step S8, the method for preparing the positive electrode sheet includes: S81, mixing and slurrying a positive electrode material, a positive electrode binder, a conductive agent and a solvent to obtain a positive electrode slurry; S82, coating the positive electrode slurry, and rolling and cutting to obtain a negative electrode positive electrode sheet; Preferably, in step S8, the method for preparing the negative electrode sheet includes: S83, mixing and slurrying the negative electrode material, the negative electrode binder, the conductive agent and the solvent to obtain a negative electrode slurry; S84, coating the negative electrode slurry, and obtaining the negative electrode sheet after rolling and cutting.