Experimental method for adsorbing cadmium ions by using modified sorghum straws
Adsorbents were prepared through multi-step treatment of modified sorghum straw, which solved the problem of cadmium ion treatment in liquor wastewater, and achieved efficient and environmentally friendly cadmium ion adsorption effect, indicating that modified sorghum straw adsorbents have significant adsorption in cadmium ion treatment. Ability and removal effects.
Patent Information
- Application Number
- CN202411228971.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-08
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
AI Technical Summary
There are difficulties in treating cadmium ions in wastewater in liquor production. The existing technology requires an effective, low-cost and environmentally friendly method to adsorb cadmium ions to protect the environment and human health.
By grinding, alkalizing, impregnation, pH adjustment, oxidation treatment and crosslinking treatment of modified sorghum straw, adsorbents with high adsorption properties are prepared, and cross-linked network structures are formed through ion exchange to improve the adsorption capacity of cadmium ions .
Modified sorghum straw adsorbent significantly improves the adsorption rate and equilibrium adsorption amount of cadmium ions, increases the surface roughness, and changes in the pore structure enhances the adsorption capacity. The exchange reaction between calcium ions and cadmium ions effectively removes cadmium ions, achieving efficient cadmium Ion treatment.
Smart Images

Figure CN119064298A_ABST
Abstract
Description
[0001] This application claims the priority of the Chinese patent application filed with the China Patent Office on September 8, 2023, with application number 202311159924.1 and application name “Experimental method for adsorption of cadmium ions by modified sorghum straw”, the entire contents of which are incorporated by reference in this application. Technical Field
[0002] The invention relates to the technical field of heavy metal adsorption, and in particular to an experimental method for adsorbing cadmium ions by modified sorghum straw. Background Art
[0003] Sorghum, also known as millet and reed millet, will be picked for liquor production after it matures, but this will produce a large amount of sorghum straw, which will be used as feed or to fill septic tanks and produce methane for fuel.
[0004] At the same time, with the development of science and technology and the progress of the times, the liquor industry has made great strides. Wastewater discharge in the liquor industry has become a thorny problem. Directly discharging wastewater into the river will cause damage and pollution to the water ecosystem in the river. The most harmful to humans in the wastewater is heavy metal ions. Once it enters the human body, it will cause harm to the body. Therefore, it has become a problem to solve the solid waste in liquor production and recycle the solid waste to adsorb heavy metals in sewage. The treatment methods of heavy metal cadmium ions in wastewater are different, and they exist in different environments. The adsorption method is flexible and simple, low-cost, high-performance, strong anti-pollution, easy to operate, and no new harmful substances will be produced during the adsorption process, avoiding the generation of secondary pollution. Therefore, there is an urgent need for an adsorption method for adsorbing cadmium ions in wastewater to verify the adsorption of modified sorghum straw on cadmium ions. Summary of the invention
[0005] The invention aims to provide an experimental method for adsorbing cadmium ions by modified sorghum straw, so as to verify the adsorption of cadmium ions in wastewater by modified sorghum straw.
[0006] In order to solve the above technical problems, the present invention provides the following technical solution: an experimental method for adsorption of cadmium ions by modified sorghum straw, comprising the following steps:
[0007] Step 1, grinding: drying the sorghum stalks and adding them into a grinding machine for grinding to obtain sorghum stalk powder;
[0008] Step 2, alkalization: adding sodium hydroxide solution to the straw powder and stirring continuously to destroy the surface layer of the sorghum straw and remove the cuticle;
[0009] Step 3, impregnation: adding an alkaline solution to the alkalized straw powder in step 2 to impregnate it;
[0010] Step 4, pH adjustment: adjusting the pH of the straw powder soaked in step 3 to a neutral pH;
[0011] Step 5, centrifugation: putting the straw powder adjusted to neutral pH in step 4 into a centrifuge for centrifugation, and separating and filtering the straw powder;
[0012] Step 6, drying: putting the separated and filtered straw powder into a dryer for drying, and after drying, obtaining alkalized sorghum straw;
[0013] Step 7, oxidation treatment: put the alkalized sorghum stalks in step 6 into a mortar and grind them into powder, then take 10-15g of the powder, add 50-75ml of pure alcohol to the powder and mix for 10 minutes at a temperature of 45°C to obtain a mixture of sorghum stalks and alcohol; put 5g of sodium periodate in a brown bottle, then add 40ml of pure water, and after the sodium periodate is completely dissolved, obtain a sodium periodate aqueous solution; use a dropper to draw the mixture of sorghum stalks and alcohol, add the mixture dropwise into the sodium periodate aqueous solution and stir for 15-20 minutes, then adjust the pH value to 4 with concentrated hydrochloric acid, wait for it to react for 12h, and after the reaction is completed, add 5ml of ethylene glycol to obtain solution A;
[0014] 50 ml of ethanol and 40 ml of water were mixed to obtain an ethanol solution, solution A was added to the ethanol solution, and the mixture was stirred and filtered to obtain a filter cake. After the filtration, the filter cake was washed with ethanol to remove the water in the filter cake, and then the filter cake was air-dried to obtain oxidized sorghum straw.
[0015] Step 8, modification treatment: take 2g of the oxidized sorghum straw obtained in step 7, add it to 30ml of alcohol and stir it at room temperature for 2 hours, then pour the solution into a round-bottom flask, add 2g of salicylic hydrazide and 5 drops of glacial acetic acid into the round-bottom flask, condense for 24h, add alcohol after condensation and filter it, then put the filtered straw into a fume hood for drying, and obtain modified sorghum straw after drying;
[0016] Step nine, finished product: weigh 2g of modified sorghum straw, weigh 0.5g of sodium alginate and dissolve them in 100ml of water, and stir until completely dissolved, then add the modified sorghum straw, add 1ml of BDE cross-linking agent after the sorghum straw is dissolved, stir for 12h, then put it in a refrigerator and freeze it for 12h, and then dry it in a freeze dryer to obtain the prepared adsorbent;
[0017] Take an appropriate amount of the prepared adsorbent and place it in 100 mL of 5% calcium chloride aqueous solution for ion exchange; stir for 3 hours, let it stand for 12 hours, filter it, and wash it with pure water 5 times to wash away the free calcium ions on the surface of the adsorbent and the Na in the sodium alginate in the functional group. +Ca 2+ Replacement, forming a cross-linked structure, increasing the cross-linked network structure of the adsorbent, and at the same time dissolving the impurities, and then placed in a refrigerator for 6 hours, and then placed in a freeze dryer for 2 days to obtain the final adsorbent;
[0018] Step 10, verification: weigh out 275.5 mg of cadmium nitrate and dissolve it in water in a 1000 mL volumetric flask to prepare a 1000 mg / L cadmium ion solution. Under different conditions, quantitatively add Cd 2+ The solution was added to the final adsorbent obtained in step nine, and the adsorbent was shaken at a speed of 180 r / min in a constant temperature oscillating box. After waiting for the adsorption time to be reached, the filtrate was filtered and the Cd in the filtrate was analyzed by AAS. 2+ The residual concentration of Cd in modified sorghum straw was measured. 2+ The removal rate of Cd was analyzed by using formula 1 and formula 2. 2+ The adsorption rate (R, %) and equilibrium adsorption capacity were calculated:
[0019] R e (%)=(C o -C e ) / C o *100% (Formula 1);
[0020] qe=(C o -C e ) / W (Formula 2);
[0021] In the above formula, Co – the initial concentration of cadmium in the solution in mg / L;
[0022] Ce——When Cd2+ reaches an equilibrium state in the solution, it is expressed in mg / L;
[0023] V——real volume of cadmium ion solution in L;
[0024] W——The weight of the improved sorghum straw absorbent is in g.
[0025] Furthermore, the concentration of the sodium hydroxide solution in step 2 is 0.1 mol / L to 0.5 mol / L.
[0026] Furthermore, during the stirring in step 2, the stirring temperature is 40 to 45° C., and the stirring time is 6 to 8 hours.
[0027] Furthermore, during the centrifugation in step five, the speed of the centrifuge is 3000 r / min.
[0028] Furthermore, when drying is performed in step six, the drying temperature is 35 to 45° C. and the drying time is 12 to 18 hours.
[0029] The working principle and beneficial effects of the present invention: The surface tissue morphology and composition of the sample before and after absorption were analyzed using scanning electron microscopy and energy spectrum technology. On the surface, the sorghum straw after alkaline hydrolysis is flaky and layered, and SEM shows that the surface of the straw is smooth, fine and has no pores. The modified sorghum straw adsorbent has a messy, rough and fine strip appearance. The results show that the surface of the material is irregular and the pore distribution is uneven. After adsorbing heavy metal cadmium ions, the roughness of the adsorbent surface increases, the pore structure inside the adsorbent decreases, and the pore stiffness increases. Under the action of hydrazone and carboxyl groups, Cd 2+ After being adsorbed, the microstructure of its surface will change significantly. Inside the channel, the opening size and smoothness of the opening are quite different. This is because under the action of cadmium, the internal structure of the modified sorghum straw has been reshaped. 2+ The overlap of EDX spectra before and after the adsorption showed that sorghum straw contained three components, C, O and Na, with their respective weight percentages of 59.56%, 30.64% and 9.80%. The modified sorghum straw adsorbent was found to have C, N, O, Na and Ca, with the weight percentages of each element being 32.55%, 23.22%, 8.17%, 2.94% and 33.12%, respectively. 2+ After that, its elemental composition became C, N, O, and Cd, and the weight percentage of each element was 27.62%, 3.84%, 1.25%, and 67.29%. Through the analysis of the test results, it was shown that under alkaline conditions, calcium ions can completely replace sodium ions, and sodium ions can be used as improved adsorbents. The results showed that in the treated sorghum straw, Ca 2+ By using Cd 2+ The EDX spectrum shows that Ca 2+ Being Cd 2+ In addition, Ca 2+ with cd 2+ An ion exchange reaction occurs, which is Ca 2+ In the role of the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the SEM spectrum of the modified sorghum straw adsorbent in the embodiment;
[0031] Figure 2 It is the EDAX spectrum of sorghum straw in the embodiment. DETAILED DESCRIPTION
[0032] Example 1
[0033] The experimental method for adsorption of cadmium ions by modified sorghum straw comprises the following steps:
[0034] Step 1, grinding: drying the sorghum stalks and adding them into a grinding machine for grinding to obtain sorghum stalk powder;
[0035] Step 2, alkalization: adding a sodium hydroxide solution with a concentration of 0.1 mol / L to the straw powder and continuously stirring to destroy the surface layer of the sorghum straw and remove the cuticle. The stirring temperature is 40° C. and the stirring time is 6 hours.
[0036] Step 3, impregnation: adding an alkaline solution to the alkalized straw powder in step 2 to impregnate it;
[0037] Step 4, pH adjustment: adjusting the pH of the straw powder soaked in step 3 to a neutral pH;
[0038] Step 5, centrifugation: put the straw powder adjusted to neutral pH in step 4 into a centrifuge for centrifugation at a speed of 3000 r / min, and separate and filter the straw powder;
[0039] Step 6, drying: putting the separated and filtered straw powder into a dryer for drying at a temperature of 35°C for 12 hours to obtain alkalized sorghum straw;
[0040] Step 7, oxidation treatment: put the alkalized sorghum stalks in step 6 into a mortar and grind them into powder, then take 10g of the powder, add 50ml of pure alcohol to the powder and mix for 10 minutes at a temperature of 45°C to obtain a mixture of sorghum stalks and alcohol; put 5g of sodium periodate in a brown bottle, then add 40ml of pure water, and after the sodium periodate is completely dissolved, obtain a sodium periodate aqueous solution; use a dropper to draw the mixture of sorghum stalks and alcohol, add the mixture dropwise into the sodium periodate aqueous solution and stir for 15 minutes, then adjust the pH value to 4 with concentrated hydrochloric acid, wait for it to react for 12h, and after the reaction is completed, add 5ml of ethylene glycol to obtain solution A;
[0041] 50 ml of ethanol and 40 ml of water were mixed to obtain an ethanol solution, solution A was added to the ethanol solution, and the mixture was stirred and filtered to obtain a filter cake. After the filtration, the filter cake was washed with ethanol to remove the water in the filter cake, and then the filter cake was air-dried to obtain oxidized sorghum straw.
[0042] Step 8, modification treatment: take 2g of the oxidized sorghum straw obtained in step 7, add it to 30ml of alcohol and stir it at room temperature for 2 hours, then pour the solution into a round-bottom flask, add 2g of salicylic hydrazide and 5 drops of glacial acetic acid into the round-bottom flask, condense for 24h, add alcohol after condensation and filter it, then put the filtered straw into a fume hood for drying, and obtain modified sorghum straw after drying;
[0043] Step nine, finished product: weigh 2g of modified sorghum straw, weigh 0.5g of sodium alginate and dissolve them in 100ml of water, and stir until completely dissolved, then add the modified sorghum straw, add 1ml of BDE cross-linking agent after the sorghum straw is dissolved, stir for 12h, then put it in a refrigerator and freeze it for 12h, and then dry it in a freeze dryer to obtain the prepared adsorbent;
[0044] Take an appropriate amount of the prepared adsorbent and place it in 100 mL of 5% calcium chloride aqueous solution for ion exchange; stir for 3 hours, let it stand for 12 hours, filter it, and wash it with pure water 5 times to wash away the free calcium ions on the surface of the adsorbent and the Na in the sodium alginate in the functional group. + Ca 2+ Replacement, forming a cross-linked structure, increasing the cross-linked network structure of the adsorbent, and at the same time dissolving the impurities, and then placed in a refrigerator for 6 hours, and then placed in a freeze dryer for 2 days to obtain the final adsorbent;
[0045] Step 10, verification: weigh out 275.5 mg of cadmium nitrate and dissolve it in water in a 1000 mL volumetric flask to prepare a 1000 mg / L cadmium ion solution. Under different conditions, quantitatively add Cd 2+ The solution was added to the final adsorbent obtained in step nine, and the adsorbent was shaken at a speed of 180 r / min in a constant temperature oscillating box. After waiting for the adsorption time to be reached, the filtrate was filtered and the Cd in the filtrate was analyzed by AAS. 2+ The residual concentration of Cd in modified sorghum straw was measured. 2+ The removal rate of Cd was analyzed by using formula 1 and formula 2. 2+ The adsorption rate (R, %) and equilibrium adsorption capacity were calculated:
[0046] R e (%)=(C o -C e ) / C o *100% (Formula 1);
[0047] qe=(C o -C e ) / W (Formula 2);
[0048] In the above formula, Co – the initial concentration of cadmium in the solution in mg / L;
[0049] Ce——When Cd2+ reaches an equilibrium state in the solution, it is expressed in mg / L;
[0050] V——real volume of cadmium ion solution in L;
[0051] W——The weight of the improved sorghum straw absorbent is in g.
[0052] Example 2
[0053] The experimental method for adsorption of cadmium ions by modified sorghum straw comprises the following steps:
[0054] Step 1, grinding: drying the sorghum stalks and adding them into a grinding machine for grinding to obtain sorghum stalk powder;
[0055] Step 2, alkalization: adding a sodium hydroxide solution with a concentration of 0.5 mol / L to the straw powder and continuously stirring to destroy the surface layer of the sorghum straw and remove the cuticle. The stirring temperature is 45° C. and the stirring time is 8 hours.
[0056] Step 3, impregnation: adding an alkaline solution to the alkalized straw powder in step 2 to impregnate it;
[0057] Step 4, pH adjustment: adjusting the pH of the straw powder soaked in step 3 to a neutral pH;
[0058] Step 5, centrifugation: put the straw powder adjusted to neutral pH in step 4 into a centrifuge for centrifugation at a speed of 3000 r / min, and separate and filter the straw powder;
[0059] Step 6, drying: putting the separated and filtered straw powder into a dryer for drying at a temperature of 45°C for 12 to 18 hours, and obtaining alkalized sorghum straw after drying;
[0060] Step 7, oxidation treatment: put the alkalized sorghum stalks in step 6 into a mortar and grind them into powder, then take 15g of the powder, add 75ml of pure alcohol to the powder and mix for 10 minutes at a temperature of 45°C to obtain a mixture of sorghum stalks and alcohol; put 5g of sodium periodate in a brown bottle, then add 40ml of pure water, and after the sodium periodate is completely dissolved, obtain a sodium periodate aqueous solution; use a dropper to draw the mixture of sorghum stalks and alcohol, add the mixture dropwise into the sodium periodate aqueous solution and stir for 20 minutes, then adjust the pH value to 4 with concentrated hydrochloric acid, wait for it to react for 12h, and after the reaction is completed, add 5ml of ethylene glycol to obtain solution A;
[0061] 50 ml of ethanol and 40 ml of water were mixed to obtain an ethanol solution, solution A was added to the ethanol solution, and the mixture was stirred and filtered to obtain a filter cake. After the filtration, the filter cake was washed with ethanol to remove the water in the filter cake, and then the filter cake was air-dried to obtain oxidized sorghum straw.
[0062] Step 8, modification treatment: take 2g of the oxidized sorghum straw obtained in step 7, add it to 30ml of alcohol and stir it at room temperature for 2 hours, then pour the solution into a round-bottom flask, add 2g of salicylic hydrazide and 5 drops of glacial acetic acid into the round-bottom flask, condense for 24h, add alcohol after condensation and filter it, then put the filtered straw into a fume hood for drying, and obtain modified sorghum straw after drying;
[0063] Step nine, finished product: weigh 2g of modified sorghum straw, weigh 0.5g of sodium alginate and dissolve them in 100ml of water, and stir until completely dissolved, then add the modified sorghum straw, add 1ml of BDE cross-linking agent after the sorghum straw is dissolved, stir for 12h, then put it in a refrigerator and freeze it for 12h, and then dry it in a freeze dryer to obtain the prepared adsorbent;
[0064] Take an appropriate amount of the prepared adsorbent and place it in 100 mL of 5% calcium chloride aqueous solution for ion exchange; stir for 3 hours, let it stand for 12 hours, filter it, and wash it with pure water 5 times to wash away the free calcium ions on the surface of the adsorbent and the Na in the sodium alginate in the functional group. + Ca 2+ Replacement, forming a cross-linked structure, increasing the cross-linked network structure of the adsorbent, and at the same time dissolving the impurities, and then placed in a refrigerator for 6 hours, and then placed in a freeze dryer for 2 days to obtain the final adsorbent;
[0065] Step 10, verification: weigh out 275.5 mg of cadmium nitrate and dissolve it in water in a 1000 mL volumetric flask to prepare a 1000 mg / L cadmium ion solution. Under different conditions, quantitatively add Cd 2+ The solution was added to the final adsorbent obtained in step nine, and the adsorbent was shaken at a speed of 180 r / min in a constant temperature oscillating box. After waiting for the adsorption time to be reached, the filtrate was filtered and the Cd in the filtrate was analyzed by AAS. 2+ The residual concentration of Cd in modified sorghum straw was measured. 2+ The removal rate of Cd was analyzed by using formula 1 and formula 2. 2+ The adsorption rate (R, %) and equilibrium adsorption capacity were calculated:
[0066] R e (%)=(C o -C e ) / Co *100% (Formula 1);
[0067] qe=(C o -C e ) / W (Formula 2);
[0068] In the above formula, Co – the initial concentration of cadmium in the solution in mg / L;
[0069] Ce——When Cd2+ reaches an equilibrium state in the solution, it is expressed in mg / L;
[0070] V——real volume of cadmium ion solution in L;
[0071] W——The weight of the improved sorghum straw absorbent is in g.
[0072] Example 3
[0073] The experimental method for adsorption of cadmium ions by modified sorghum straw comprises the following steps:
[0074] Step 1, grinding: drying the sorghum stalks and adding them into a grinding machine for grinding to obtain sorghum stalk powder;
[0075] Step 2, alkalization: adding a sodium hydroxide solution with a concentration of 0.3 mol / L to the straw powder and continuously stirring to destroy the surface layer of the sorghum straw and remove the cuticle. The stirring temperature is 42° C. and the stirring time is 7 hours.
[0076] Step 3, impregnation: adding an alkaline solution to the alkalized straw powder in step 2 to impregnate it;
[0077] Step 4, pH adjustment: adjusting the pH of the straw powder soaked in step 3 to a neutral pH;
[0078] Step 5, centrifugation: put the straw powder adjusted to neutral pH in step 4 into a centrifuge for centrifugation at a speed of 3000 r / min, and separate and filter the straw powder;
[0079] Step 6, drying: putting the separated and filtered straw powder into a dryer for drying at a temperature of 35-45°C for 15 hours to obtain alkalized sorghum straw;
[0080] Step 7, oxidation treatment: put the alkalized sorghum stalks in step 6 into a mortar and grind them into powder, then take 10-15g of the powder, add 65ml of pure alcohol to the powder and mix for 10 minutes at a temperature of 45°C to obtain a mixture of sorghum stalks and alcohol; put 5g of sodium periodate in a brown bottle, then add 40ml of pure water, and after the sodium periodate is completely dissolved, obtain a sodium periodate aqueous solution; use a dropper to draw the mixture of sorghum stalks and alcohol, add the mixture dropwise into the sodium periodate aqueous solution and stir for 18 minutes, then adjust the pH value to 4 with concentrated hydrochloric acid, wait for it to react for 12h, and after the reaction is completed, add 5ml of ethylene glycol to obtain solution A;
[0081] 50 ml of ethanol and 40 ml of water were mixed to obtain an ethanol solution, solution A was added to the ethanol solution, and the mixture was stirred and filtered to obtain a filter cake. After the filtration, the filter cake was washed with ethanol to remove the water in the filter cake, and then the filter cake was air-dried to obtain oxidized sorghum straw.
[0082] Step 8, modification treatment: take 2g of the oxidized sorghum straw obtained in step 7, add it to 30ml of alcohol and stir it at room temperature for 2 hours, then pour the solution into a round-bottom flask, add 2g of salicylic hydrazide and 5 drops of glacial acetic acid into the round-bottom flask, condense for 24h, add alcohol after condensation and filter it, then put the filtered straw into a fume hood for drying, and obtain modified sorghum straw after drying;
[0083] Step nine, finished product: weigh 2g of modified sorghum straw, weigh 0.5g of sodium alginate and dissolve them in 100ml of water, and stir until completely dissolved, then add the modified sorghum straw, add 1ml of BDE cross-linking agent after the sorghum straw is dissolved, stir for 12h, then put it in a refrigerator and freeze it for 12h, and then dry it in a freeze dryer to obtain the prepared adsorbent;
[0084] Take an appropriate amount of the prepared adsorbent and place it in 100 mL of 5% calcium chloride aqueous solution for ion exchange; stir for 3 hours, let it stand for 12 hours, filter it, and wash it with pure water 5 times to wash away the free calcium ions on the surface of the adsorbent and the Na in the sodium alginate in the functional group. + Ca 2+ Replacement, forming a cross-linked structure, increasing the cross-linked network structure of the adsorbent, and at the same time dissolving the impurities, and then placed in a refrigerator for 6 hours, and then placed in a freeze dryer for 2 days to obtain the final adsorbent;
[0085] Step 10, verification: weigh out 275.5 mg of cadmium nitrate and dissolve it in water in a 1000 mL volumetric flask to prepare a 1000 mg / L cadmium ion solution. Under different conditions, quantitatively add Cd 2+The solution was added to the final adsorbent obtained in step nine, and the adsorbent was shaken at a speed of 180 r / min in a constant temperature oscillating box. After waiting for the adsorption time to be reached, the filtrate was filtered and the Cd in the filtrate was analyzed by AAS. 2+ The residual concentration of Cd in modified sorghum straw was measured. 2+ The removal rate of Cd was analyzed by using formula 1 and formula 2. 2+ The adsorption rate (R, %) and equilibrium adsorption capacity were calculated:
[0086] R e (%)=(C o -C e ) / C o *100% (Formula 1);
[0087] qe=(C o -C e ) / W (Formula 2);
[0088] In the above formula, Co – the initial concentration of cadmium in the solution in mg / L;
[0089] Ce——When Cd2+ reaches an equilibrium state in the solution, it is expressed in mg / L;
[0090] V——real volume of cadmium ion solution in L;
[0091] W——The weight of the improved sorghum straw absorbent is in g.
[0092] By the attached Figure 1 It can be seen that the surface morphology and composition of the samples before and after absorption were analyzed by scanning electron microscopy and energy spectrum technology. On the surface, the sorghum straw after alkaline hydrolysis is flaky and layered. SEM shows that the surface of the straw is smooth, dense and has no pores ( Figure 1 The modified sorghum straw adsorbent has a messy, rough, and fine stripe appearance ( Figure 1 The results show that the surface of the material is irregular and the pore distribution is uneven. After adsorbing heavy metal cadmium ions, the roughness of the adsorbent surface increases, the pore structure inside the adsorbent decreases, and the pore stiffness increases ( Figure 1 , left figure).
[0093] By the attached Figure 2The results in the study showed that sorghum straw contained three components, C, O and Na, with respective weight percentages of 59.56%, 30.64% and 9.80%. The modified sorghum straw adsorbent was found to have C, N, O, Na and Ca, with the weight percentages of each element being 32.55%, 23.22%, 8.17%, 2.94% and 33.12%, respectively. After absorbing Cd2+, its elemental composition became C, N, O, Cd, with the weight percentages of each element being 27.62%, 3.84%, 1.25%, 67.29%. By analyzing the test results, it was shown that under alkaline conditions, calcium ions could completely replace sodium ions, while sodium ions could serve as the modified adsorbent. The results showed that in the treated sorghum straw, Ca2+ was removed by ion exchange with Cd2+. The EDX spectrum showed that Ca2+ was completely replaced by Cd2+. In addition, Ca2+ and Cd2+ underwent ion exchange reaction.
Claims
1. The experimental method for adsorption of cadmium ions by modified sorghum straw is characterized by: The experimental method for adsorption of cadmium ions by modified sorghum straw comprises the following steps: Step 1, grinding: drying the sorghum stalks and adding them into a grinding machine for grinding to obtain sorghum stalk powder; Step 2, alkalization: adding sodium hydroxide solution to the straw powder and stirring continuously to destroy the surface layer of the sorghum straw and remove the cuticle; Step 3, impregnation: adding an alkaline solution to the alkalized straw powder in step 2 to impregnate it; Step 4, pH adjustment: adjusting the pH of the straw powder soaked in step 3 to a neutral pH; Step 5, centrifugation: putting the straw powder adjusted to neutral pH in step 4 into a centrifuge for centrifugation, and separating and filtering the straw powder; Step 6, drying: putting the separated and filtered straw powder into a dryer for drying, and after drying, obtaining alkalized sorghum straw; Step 7, oxidation treatment: put the alkalized sorghum stalks in step 6 into a mortar and grind them into powder, then take 10-15g of the powder, add 50-75ml of pure alcohol to the powder and mix for 10 minutes at a temperature of 45°C to obtain a mixture of sorghum stalks and alcohol; put 5g of sodium periodate in a brown bottle, then add 40ml of pure water, and after the sodium periodate is completely dissolved, obtain a sodium periodate aqueous solution; use a dropper to draw the mixture of sorghum stalks and alcohol, add the mixture dropwise into the sodium periodate aqueous solution and stir for 15-20 minutes, then adjust the pH value to 4 with concentrated hydrochloric acid, wait for it to react for 12h, and after the reaction is completed, add 5ml of ethylene glycol to obtain solution A; 50 ml of ethanol and 40 ml of water were mixed to obtain an ethanol solution, solution A was added to the ethanol solution, and the mixture was stirred and filtered to obtain a filter cake. After the filtration, the filter cake was washed with ethanol to remove the water in the filter cake, and then the filter cake was air-dried to obtain oxidized sorghum straw. Step 8, modification treatment: take 2g of the oxidized sorghum straw obtained in step 7, add it to 30ml of alcohol and stir it at room temperature for 2 hours, then pour the solution into a round-bottom flask, add 2g of salicylic hydrazide and 5 drops of glacial acetic acid into the round-bottom flask, condense for 24h, add alcohol after condensation and filter it, then put the filtered straw into a fume hood for drying, and obtain modified sorghum straw after drying; Step nine, finished product: weigh 2g of modified sorghum straw, weigh 0.5g of sodium alginate and dissolve them in 100ml of water, and stir until completely dissolved, then add the modified sorghum straw, add 1ml of BDE cross-linking agent after the sorghum straw is dissolved, stir for 12h, then put it in a refrigerator and freeze it for 12h, and then dry it in a freeze dryer to obtain the prepared adsorbent; Step 10, verification: weigh out 275.5 mg of cadmium nitrate and dissolve it in water in a 1000 mL volumetric flask to prepare a 1000 mg / L cadmium ion solution. Under different conditions, quantitatively add Cd 2+ The solution was added to the adsorbent obtained in step nine, and the adsorbent was shaken at a speed of 180 r / min in a constant temperature oscillating box. After waiting for the adsorption time to be reached, the filtrate was filtered and the Cd in the filtrate was analyzed by AAS. 2+ The residual concentration of Cd in modified sorghum straw was measured. 2+ The removal rate of Cd was analyzed by using formula 1 and formula 2. 2+ The adsorption rate (R, %) and equilibrium adsorption capacity were calculated: R e (%)=(C o -C e ) / C o *100% (Formula 1); qe=(C o -C e ) / W (Formula 2); In the above formula, Co – the initial concentration of cadmium in the solution in mg / L; Ce——When Cd2+ reaches an equilibrium state in the solution, it is expressed in mg / L; V——the actual volume of the cadmium ion solution in L; W——The weight of the improved sorghum straw absorbent is in g.
2. The method for adsorption of cadmium ions by modified sorghum straw according to claim 1, characterized in that: The sodium hydroxide solution in step 2 has a concentration of 0.1 mol / L to 0.5 mol / L.
3. The experimental method for adsorption of cadmium ions by modified sorghum straw according to claim 2, characterized in that: When stirring in step 2, the stirring temperature is 40-45° C. and the stirring time is 6-8 hours.
4. The experimental method for adsorption of cadmium ions by modified sorghum straw according to claim 3, characterized in that: During the centrifugation in step 5, the speed of the centrifuge is 3000 r / min.
5. The experimental method for adsorption of cadmium ions by modified sorghum straw according to claim 4, characterized in that: When drying is performed in step six, the drying temperature is 35 to 45° C. and the drying time is 12 to 18 hours.