Method for manufacturing polarizing plate

By applying acidic aqueous solution on the polarizing film and multi-stage stretching treatment, the durability problem of the polarizing film in high temperature and high humidity environment is solved, and a polarizing plate with high single-piece transmission and excellent durability is achieved, which is suitable for thinning. Image display device.

CN119065047APending Publication Date: 2024-12-03NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411088324.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-06-25
Filing Date
2020-06-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing polarizing film has insufficient durability in high temperature and high humidity environments, making it difficult to meet the needs of thin-format image display devices.

Method used

An acidic aqueous solution containing an acid component and a pH of 2.5 or less was applied to the surface of the polarizing film, and combined with multi-stage stretching and drying shrinkage treatment, a polarizing plate with high single-piece transmittance and excellent durability was formed.

Benefits of technology

The durability and optical characteristics of the polarizer in high temperature and high humidity environment are significantly improved, and the stability and performance of the thinner image display device are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119065047A_ABST
    Figure CN119065047A_ABST
Patent Text Reader

Abstract

Provided are: a polarizing plate which has high single-sheet transmittance and excellent durability in a high-temperature and high-humidity environment; and a method for producing the polarizing plate. This method for manufacturing a polarizing plate includes applying an acidic aqueous solution containing an acid component and having a pH of 2.5 or less to at least one surface of a polarizing film.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This case is a divisional application of an application with a filing date of June 19, 2020, application number 202080046164.1, and invention name “Method for manufacturing a polarizing plate”. Technical Field

[0002] The present invention relates to a method for manufacturing a polarizing plate. Background Art

[0003] In a liquid crystal display device, which is a representative image display device, polarizing films are arranged on both sides of the liquid crystal unit due to its image forming method. As a method for manufacturing a polarizing film, for example, the following method is proposed: a laminate having a resin substrate and a polyvinyl alcohol-based resin layer is stretched, and then dyed to obtain a polarizing film on the resin substrate (for example, Patent Document 1). According to this method, a polarizing film with a thinner thickness can be obtained, and therefore, it has attracted attention because it contributes to the thinning of image display devices in recent years. However, for thin polarizing films, further improvement of durability in high temperature and high humidity environments is sought.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2001-343521 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide a method for producing a polarizing plate having high single-piece transmittance and excellent durability in a high-temperature and high-humidity environment.

[0009] Solutions for solving problems

[0010] According to one aspect of the present invention, there is provided a method for manufacturing a polarizing plate, the method comprising: applying an acidic aqueous solution containing an acid component and having a pH of 2.5 or less to at least one surface of a polarizing film.

[0011] In one embodiment, the acid component includes hydrogen chloride.

[0012] In one embodiment, the acid component includes sulfuric acid.

[0013] In one embodiment, the acidic aqueous solution further includes a water-soluble resin, which is applied to at least one surface of the polarizing film and dried to form a functional film.

[0014] In one embodiment, the water-soluble resin includes a polyvinyl alcohol-based resin.

[0015] In one embodiment, the degree of polymerization of the polyvinyl alcohol-based resin is 1500 to 4500.

[0016] In one embodiment, the acidic aqueous solution has a viscosity of 350 mPa·sec or less.

[0017] Effects of the Invention

[0018] The manufacturing method of the present invention includes applying an acidic aqueous solution having a predetermined pH to the surface of a polarizing film. According to this manufacturing method, a polarizing plate having a high single-piece transmittance and excellent durability in a high-temperature and high-humidity environment can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram showing an example of a drying and shrinking process using a heating roller.

[0020] Figure 2 This is a schematic cross-sectional view of an example of a polarizing plate obtained by the production method of the present invention.

[0021] Figure 3 This is a schematic cross-sectional view of another example of a polarizing plate obtained by the production method of the present invention. DETAILED DESCRIPTION

[0022] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0023] A. Method for manufacturing polarizing plate

[0024] The method for manufacturing a polarizing plate according to an embodiment of the present invention includes applying an acidic aqueous solution containing an acid component and having a pH of 2.5 or less to at least one surface of a polarizing film. By applying the acidic aqueous solution to the surface, the durability of the polarizing film in a high temperature and high humidity environment can be improved.

[0025] The polarizing film included in the polarizing plate can be made using a single polyvinyl alcohol (PVA) resin film, or can be made using a laminate of two or more layers including a PVA resin layer. As a specific example of a polarizing film obtained using a laminate, a polarizing film obtained using a laminate of a thermoplastic resin substrate and a PVA resin layer formed on the thermoplastic resin substrate by coating can be cited.

[0026] A-1. Method for producing a polarizing plate using a laminate

[0027] The manufacturing method of the polarizing plate described in one embodiment of the present invention includes: forming a PVA-based resin layer on one side of a long thermoplastic resin substrate to form a laminate; stretching and dyeing the laminate to make the PVA-based resin layer into a polarizing film; and applying an acidic aqueous solution containing an acid component and a pH of 2.5 or less to at least one surface of the polarizing film. In this embodiment, it is preferred that the PVA-based resin layer is made into a polarizing film by sequentially subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, and an underwater stretching treatment. In addition, the PVA-based resin layer preferably contains a halide and a PVA-based resin. The manufacturing method may also include the following drying and shrinking treatment: the laminate after the underwater stretching treatment is heated while being conveyed along the length direction, so that it shrinks by more than 2% in the width direction. The drying and shrinking treatment is preferably performed using a heating roller, and the temperature of the heating roller is preferably 60°C to 120°C. In particular, by preparing a laminate including a PVA-based resin layer and the PVA-based resin layer including a halide and a PVA-based resin, setting the stretching of the laminate to a multi-stage stretching including an air auxiliary stretching and an underwater stretching, and heating the stretched laminate with a heating roller, a polarizing film having excellent optical properties (typically, single-sheet transmittance and polarization degree) can be obtained. When the method for manufacturing a polarizing plate includes a drying shrinkage treatment, the application of the acidic aqueous solution can be performed after the underwater stretching treatment and before the drying shrinkage treatment, or after the drying shrinkage treatment.

[0028] A-1-1. Preparation of laminate

[0029] As a method for preparing a laminate of a thermoplastic resin substrate and a PVA-based resin layer, any appropriate method may be adopted. Preferably, a coating liquid containing a PVA-based resin is applied to the surface of the thermoplastic resin substrate and dried to form the PVA-based resin layer on the thermoplastic resin substrate.

[0030] Any appropriate method may be used for applying the coating liquid, such as roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.). The coating / drying temperature of the coating liquid is preferably 50° C. or higher.

[0031] The thickness of the PVA-based resin layer is preferably 3 μm to 40 μm, more preferably 3 μm to 20 μm.

[0032] Before forming the PVA based resin layer, the thermoplastic resin substrate may be subjected to a surface treatment (e.g., corona treatment) or an easy-adhesive layer may be formed on the thermoplastic resin substrate. By carrying out such treatment, the adhesion between the thermoplastic resin substrate and the PVA based resin layer can be improved.

[0033] As the thermoplastic resin substrate, any and appropriate thermoplastic resin film can be used. The details of the thermoplastic resin substrate are recorded in, for example, Japanese Patent Publication No. 2012-73580. The entire record of the publication is cited in this specification as a reference. Preferably, a polyester resin is used, and more preferably, a polyethylene terephthalate resin is used.

[0034] The coating liquid contains a PVA resin and preferably further contains a halide. The coating liquid may be, for example, a solution obtained by dissolving a halide and a PVA resin in a solvent. As the solvent, for example, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyols such as trimethylolpropane, amines such as ethylenediamine and diethylenetriamine may be cited. They may be used alone or in combination of two or more. Among these, the solvent is preferably water.

[0035] As the above-mentioned PVA-based resin, any and appropriate resin can be used. For example, polyvinyl alcohol and ethylene-vinyl alcohol copolymer can be listed. Polyvinyl alcohol can be obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer can be obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of PVA-based resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be obtained according to JIS K 6726-1994. By using a PVA-based resin with such a saponification degree, a polarizing film with excellent durability can be obtained. When the saponification degree is too high, gelation is likely to occur.

[0036] The average degree of polymerization of the PVA-based resin can be appropriately selected depending on the purpose. The average degree of polymerization is usually 1000 to 10000, preferably 1200 to 4500, and more preferably 1500 to 4300. The average degree of polymerization can be determined according to JIS K 6726-1994.

[0037] The PVA resin preferably includes an acetoacetyl-modified PVA resin. If this is the structure, a polarizing film with desired mechanical strength can be obtained. When the PVA resin as a whole is set to 100 wt %, the blending amount of the acetoacetyl-modified PVA resin is preferably 5 wt % to 20 wt %, and more preferably 8 wt % to 12 wt %. If the blending amount is in this range, a polarizing film with more excellent mechanical strength can be obtained.

[0038] The concentration of the PVA-based resin in the coating liquid is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is closely attached to the thermoplastic resin substrate can be formed.

[0039] As the above-mentioned halide, any appropriate halide can be used. Examples thereof include iodide and sodium chloride. As the iodide, examples thereof include potassium iodide, sodium iodide and lithium iodide. Among these, potassium iodide is preferred.

[0040] The amount of the halide in the coating liquid is preferably 5 to 20 parts by weight, more preferably 10 to 15 parts by weight, based on 100 parts by weight of the PVA resin. If the amount of the halide exceeds 20 parts by weight, the halide may ooze out, and the polarizing film finally obtained may become turbid.

[0041] Generally speaking, the orientation of the polyvinyl alcohol molecules in the PVA resin increases due to the stretching of the PVA resin layer, but when the stretched PVA resin layer is immersed in a liquid containing water, the orientation of the polyvinyl alcohol molecules is sometimes disordered and the orientation decreases. In particular, when a laminate of a thermoplastic resin substrate and a PVA resin layer is stretched in boric acid water, the orientation tends to decrease significantly when the laminate is stretched in boric acid water at a higher temperature in order to stabilize the stretching of the thermoplastic resin substrate. For example, the stretching of a PVA film alone in boric acid water is usually carried out at 60°C. In contrast, the stretching of a laminate of A-PET (thermoplastic resin substrate) and a PVA resin layer is carried out at a high temperature of about 70°C. At this time, the orientation of the PVA at the initial stage of stretching may decrease before it rises due to the stretching in water. In contrast, by preparing a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate, and stretching the laminate at a high temperature in air (auxiliary stretching) before stretching the laminate in boric acid water, the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-based resin layer does not contain a halide. Thus, the optical properties of the polarizing film obtained by the treatment process of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved.

[0042] Additives may be further compounded into the coating liquid. Examples of additives include plasticizers and surfactants. Examples of plasticizers include polyols such as ethylene glycol and glycerol. Examples of surfactants include nonionic surfactants. These may be used to further improve the uniformity, dyeability, and stretchability of the resulting PVA-based resin layer.

[0043] A-1-2. Aerial assisted stretching

[0044] In particular, in order to obtain high optical properties, a two-stage stretching method combining dry stretching (auxiliary stretching) and underwater stretching (preferably boric acid underwater stretching) can be selected. By introducing auxiliary stretching as in two-stage stretching, it is possible to stretch while suppressing the crystallization of the thermoplastic resin substrate, and it is possible to solve the problem of reduced stretchability due to excessive crystallization of the thermoplastic resin substrate in subsequent underwater stretching (preferably boric acid underwater stretching), and the laminate can be stretched to a higher ratio. Furthermore, when applying PVA-based resin on a thermoplastic resin substrate, in order to suppress the influence of the glass transition temperature of the thermoplastic resin substrate, it is necessary to reduce the coating temperature compared to the usual case of applying PVA-based resin on a metal roller, and as a result, the crystallization of the PVA-based resin may be relatively low and the problem of being unable to obtain sufficient optical properties may occur. In contrast, by introducing auxiliary stretching, even when applying PVA-based resin on a thermoplastic resin substrate, the crystallinity of the PVA-based resin can be improved, and high optical properties can be achieved. Furthermore, by improving the orientation of the PVA-based resin in advance, it is possible to prevent problems such as a decrease in orientation and dissolution of the PVA-based resin when immersed in water in the subsequent dyeing and stretching steps, thereby achieving high optical properties.

[0045] The stretching method of aerial auxiliary stretching can be fixed-end stretching (for example, a method of stretching using a tenter stretching machine) or free-end stretching (for example, a method of uniaxially stretching the laminate by passing it between rollers with different circumferential speeds). In order to obtain high optical properties, free-end stretching can be actively adopted. In one embodiment, the aerial stretching process includes a heating roller stretching process in which the above-mentioned laminate is stretched while being transported along its length direction using the circumferential speed difference between the heating rollers. Representatively, the aerial stretching process includes a regional stretching process and a heating roller stretching process. It should be noted that the order of the regional stretching process and the heating roller stretching process is not limited. The regional stretching process can be performed first, or the heating roller stretching process can be performed first. The regional stretching process can also be omitted. In one embodiment, the regional stretching process and the heating roller stretching process are performed in sequence. In addition, in other embodiments, in the tenter stretching machine, stretching is performed by holding the end of the film and widening the distance between the tenters along the flow direction (the expansion of the distance between the tenters becomes the stretching ratio). At this time, the distance of the tenters in the width direction (the direction perpendicular to the flow direction) is set in an arbitrarily close manner. It is preferable to set the stretch ratio in the flow direction in a manner closer to free-end stretching. In the case of free-end stretching, the shrinkage ratio in the width direction = (1 / stretch ratio) 1 / 2 to calculate.

[0046] The auxiliary stretching in the air can be carried out in one stage or in multiple stages. When it is carried out in multiple stages, the stretching ratio is the product of the stretching ratios of each stage. The stretching direction in the auxiliary stretching in the air is preferably substantially the same as the stretching direction in the underwater stretching.

[0047] The stretching ratio in the air auxiliary stretching is preferably 2.0 to 3.5 times. The maximum stretching ratio when the air auxiliary stretching is combined with the underwater stretching is preferably 5.0 times or more, more preferably 5.5 times or more, and further preferably 6.0 times or more relative to the original length of the laminate. In this specification, the "maximum stretching ratio" refers to the stretching ratio before the laminate is about to break, and refers to the stretching ratio at which the laminate is separately confirmed to break, and is 0.2 lower than its value.

[0048] The stretching temperature of the aerial auxiliary stretching can be set to any and appropriate value according to the forming material of the thermoplastic resin substrate, the stretching method, etc. The stretching temperature is preferably above the glass transition temperature (Tg) of the thermoplastic resin substrate, more preferably above the glass transition temperature (Tg) of the thermoplastic resin substrate + 10 ° C, and particularly preferably above Tg + 15 ° C. On the other hand, the upper limit of the stretching temperature is preferably 170 ° C. By stretching at such a temperature, the crystallization of the PVA-based resin can be suppressed from proceeding rapidly, and the adverse conditions caused by the crystallization (for example, hindering the orientation of the PVA-based resin layer achieved by stretching) can be suppressed.

[0049] A-1-3. Insolubilization, dyeing and cross-linking

[0050] As needed, after the auxiliary stretching treatment in the air and before the stretching treatment in the water and the dyeing treatment, an insolubilization treatment is performed. Typically, the insolubilization treatment is performed by immersing the PVA-based resin layer in an aqueous boric acid solution. Typically, the dyeing treatment is performed by dyeing the PVA-based resin layer with iodine. As needed, after the dyeing treatment and before the stretching treatment in the water, a crosslinking treatment is performed. Typically, the crosslinking treatment is performed by immersing the PVA-based resin layer in an aqueous boric acid solution. Details of the insolubilization treatment, the dyeing treatment, and the crosslinking treatment are described, for example, in Japanese Patent Gazette No. 2012-73580.

[0051] A-1-4. Underwater stretching

[0052] The underwater stretching treatment is performed by immersing the laminate in a stretching bath. According to the underwater stretching treatment, the laminate can be stretched at a temperature lower than the glass transition temperature (typically, about 80° C.) of the thermoplastic resin substrate and the PVA-based resin layer, and the PVA-based resin layer can be stretched to a high ratio while suppressing its crystallization. As a result, a polarizing film with excellent optical properties can be manufactured.

[0053] The stretching method of the laminate can be any and appropriate method. Specifically, it can be fixed end stretching or free end stretching (for example, a method of uniaxially stretching the laminate by passing the laminate between rollers with different circumferential speeds). Preferably, free end stretching is selected. The stretching of the laminate can be carried out in one stage or in multiple stages. When it is carried out in multiple stages, the stretching ratio (maximum stretching ratio) of the laminate described later is the product of the stretching ratios of each stage.

[0054] The underwater stretching is preferably performed by immersing the laminate in an aqueous solution of boric acid (boric acid underwater stretching). By using an aqueous solution of boric acid as a stretching bath, the PVA-based resin layer can be given rigidity and water resistance that can withstand the tension applied during stretching. Specifically, boric acid can generate tetrahydroxyborate anions in an aqueous solution and cross-link with the PVA-based resin by means of hydrogen bonds. As a result, the PVA-based resin layer can be given rigidity and water resistance, thereby being well stretched, and a polarizing film with excellent optical properties can be manufactured.

[0055] The above-mentioned boric acid aqueous solution is preferably obtained by dissolving boric acid and / or a borate in water as a solvent. The boric acid concentration is preferably 1 to 10 parts by weight relative to 100 parts by weight of water, more preferably 2.5 to 6 parts by weight, and particularly preferably 3 to 5 parts by weight. By setting the boric acid concentration to 1 part by weight or more, the dissolution of the PVA-based resin layer can be effectively suppressed, and a polarizing film with higher characteristics can be manufactured. It should be noted that an aqueous solution obtained by dissolving a boron compound such as borax, glyoxal, glutaraldehyde, etc. in a solvent in addition to boric acid or a borate can also be used.

[0056] It is preferred to mix an iodide into the stretching bath (boric acid aqueous solution). By mixing an iodide, the dissolution of iodine adsorbed to the PVA-based resin layer can be suppressed. Specific examples of iodide are as described above. The concentration of iodide is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 8 parts by weight relative to 100 parts by weight of water.

[0057] The stretching temperature (liquid temperature of the stretching bath) is preferably 40°C to 85°C, more preferably 60°C to 75°C. If it is this temperature, it is possible to stretch to a high ratio while suppressing the dissolution of the PVA-based resin layer. Specifically, as described above, due to the relationship with the formation of the PVA-based resin layer, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably above 60°C. At this time, if the stretching temperature is lower than 40°C, considering the plasticization of the thermoplastic resin substrate caused by water, it may not be stretched well. On the other hand, the higher the temperature of the stretching bath, the higher the solubility of the PVA-based resin layer becomes, and it may not be possible to obtain excellent optical properties. The immersion time of the laminate in the stretching bath is preferably 15 seconds to 5 minutes.

[0058] The stretching ratio based on the underwater stretching is preferably 1.5 times or more, more preferably 3.0 times or more. The total stretching ratio of the laminate is preferably 5.0 times or more, more preferably 5.5 times or more relative to the original length of the laminate. By achieving this high stretching ratio, a polarizing film with extremely excellent optical properties can be manufactured. This high stretching ratio can be achieved by adopting an underwater stretching method (boric acid underwater stretching).

[0059] A-1-5. Cleaning

[0060] It is preferred to perform a cleaning treatment after the stretching treatment in water and before the drying shrinkage treatment. Typically, the cleaning treatment is performed by immersing the PVA-based resin layer in an aqueous solution containing an iodide such as potassium iodide. The iodide concentration in the cleaning solution is preferably 0.5 wt % to 10 wt %, preferably 0.5 wt % to 5 wt %, and more preferably 1 wt % to 4 wt %. The temperature of the cleaning solution is generally 10° C. to 50° C., preferably 20° C. to 35° C. The immersion time is generally 1 second to 1 minute, preferably 10 seconds to 1 minute.

[0061] A-1-6. Drying shrinkage treatment

[0062] The above-mentioned drying shrinkage treatment can be carried out by the regional heating carried out by the heating area as a whole, or by heating the conveying roller (using the so-called heating roller) (heating roller drying method). It is preferred to use both of them. By using a heating roller to dry it, the heating warping of the laminate can be effectively suppressed, and a polarizing film with excellent appearance is manufactured. Specifically, by drying the laminate along the state of the heating roller, the crystallization of the above-mentioned thermoplastic resin substrate can be effectively promoted to increase the crystallinity, even if the drying temperature is relatively low, the crystallinity of the thermoplastic resin substrate can be well increased. As a result, the rigidity of the thermoplastic resin substrate increases, presenting a state that can withstand the shrinkage of the PVA-based resin layer caused by drying, and warping can be suppressed. In addition, by using a heating roller, the laminate can be dried while maintaining a flat state, therefore, not only warping can be suppressed, but also the generation of wrinkles can be suppressed. At this time, the laminate is shrunk along the width direction by utilizing the drying shrinkage treatment, so that the optical properties can be improved. This is because the orientation of PVA and PVA / iodine complex can be effectively improved. The shrinkage rate of the laminate in the width direction based on the drying shrinkage treatment is preferably 2% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%. By using a heated roller, the laminate can be continuously shrunk in the width direction while being conveyed, and high productivity can be achieved.

[0063] Figure 1Schematic diagram showing an example of drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by using the transport rollers R1 to R6 and the guide rollers G1 to G4 heated to a predetermined temperature. In the example shown in the figure, the transport rollers R1 to R6 are arranged in a manner that the surface of the PVA resin layer and the surface of the thermoplastic resin substrate are alternately and continuously heated, but the transport rollers R1 to R6 may also be arranged in a manner that only one side of the laminate 200 (for example, the thermoplastic resin substrate surface) is continuously heated.

[0064] The drying conditions can be controlled by adjusting the heating temperature of the conveying roller (the temperature of the heating roller), the number of heating rollers, the contact time with the heating roller, etc. The temperature of the heating roller is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. The crystallinity of the thermoplastic resin can be increased well, warping can be suppressed well, and an optical laminate with extremely excellent durability can be manufactured. It should be noted that the temperature of the heating roller can be measured using a contact thermometer. In the example shown in the figure, 6 conveying rollers are provided, but there is no particular limitation as long as there are multiple conveying rollers. Conveying rollers are usually provided in 2 to 40 numbers, preferably 4 to 30 numbers. The contact time (total contact time) between the laminate and the heating roller is preferably 1 second to 300 seconds, more preferably 1 to 20 seconds, and more preferably 1 to 10 seconds.

[0065] The heating roller can be set in a heating furnace (such as an oven) or in a normal production line (under room temperature environment). It is preferably set in a heating furnace equipped with an air supply unit. By combining the drying based on the heating roller and the hot air drying, the rapid temperature change between the heating rollers can be suppressed, and the shrinkage in the width direction can be easily controlled. The temperature of the hot air drying is preferably 30°C to 100°C. In addition, the hot air drying time is preferably 1 second to 300 seconds. The wind speed of the hot air is preferably about 10m / s to 30m / s. It should be noted that the wind speed is the wind speed in the heating furnace and can be measured by a mini blade type digital anemometer.

[0066] A-1-7. Application of acidic aqueous solution

[0067] In one embodiment, an acidic aqueous solution containing an acid component and a pH of 2.5 or less is applied to the surface of the polarizing film of the laminate (polarizing plate) of the thermoplastic resin substrate and the polarizing film obtained as above. In this embodiment, the thermoplastic resin substrate can be directly used as a protective layer of the polarizing film. In another embodiment, a resin film (forming a protective layer) is laminated to the surface of the polarizing film of the laminate of the thermoplastic resin substrate and the polarizing film, a laminate of a protective layer / polarizing film / thermoplastic resin substrate is prepared, the thermoplastic resin substrate is peeled off from the laminate, a laminate (polarizing plate) of a protective layer / polarizing film is prepared, and the acidic aqueous solution is applied to the surface of the polarizing film of the obtained polarizing plate. After applying the above-mentioned acidic aqueous solution, another protective layer can be laminated to the side of the polarizing film where the protective layer (thermoplastic resin substrate) is not provided (the coated surface side of the acidic aqueous solution) as needed.

[0068] As the acid component contained in the above-mentioned acidic aqueous solution, any and appropriate acid can be used as long as the pH of the acidic aqueous solution can be adjusted to less than 2.5. As a specific example of the acid component, hydrogen chloride, sulfuric acid, nitric acid, phosphoric acid, citric acid, etc. can be listed, wherein, preferably strong acids such as hydrogen chloride, sulfuric acid, nitric acid (for example, acids with pKa<3), more preferably hydrogen chloride and sulfuric acid. The acid component can be used alone or in combination of two or more.

[0069] The concentration of the acid component in the acidic aqueous solution can be appropriately set in consideration of the desired pH. Typically, the pH (20°C) of the acidic aqueous solution is 2.5 or less, preferably 2.3 or less, and more preferably 2.1 or less. By applying an acidic aqueous solution having a pH of 2.5 or less, preferably 2.3 or less, to the surface of the polarizing film, when the polarizing film is exposed to a high temperature and high humidity environment, the absorbance at 600 nm, which would be reduced if it were a conventional polarizing film, can be increased (for PVA-I5 - absorption), and can suppress the absorbance at 470nm (for PVA-I3 - The absorption of the polarizing film is reduced, thereby improving the durability of the polarizing film in a high temperature and high humidity environment. It should be noted that the lower limit of the pH of the acidic aqueous solution is not particularly limited and can be set to 0.9 or more.

[0070] The acidic aqueous solution may further contain a water-soluble resin on the basis of containing an acid component. In this case, the acidic aqueous solution may be an aqueous solution obtained by dissolving an acid component and a water-soluble resin in water. By using an acidic aqueous solution containing a water-soluble resin, the acidic aqueous solution is applied to the surface of the polarizing film and dried, thereby forming a functional film containing an acid component and having a water-soluble resin as a base resin on the surface of the polarizing film. By making such a functional film exist adjacent to the polarizing film, the following results can be more suitably obtained: the result that the acid component seeps from the functional film to the polarizing film and acts in a humidified environment, and the effect of improving the durability of the polarizing film.

[0071] As the water-soluble resin, PVA resin, acrylic resin, polysulfone resin, polystyrene resin, etc. can be listed. Among them, PVA resin can be preferably used. PVA resin has excellent adhesion to polarizing film, and further, it is easy to form an aqueous solution with excellent operability, and can give appropriate mechanical strength to the obtained functional film. The water-soluble resin can be used alone or in combination of two or more.

[0072] As the above-mentioned PVA resin, any and appropriate resin can be used. For example, polyvinyl alcohol and ethylene-vinyl alcohol copolymer can be listed. Polyvinyl alcohol can be obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer can be obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of PVA resin is preferably 98.00 mol% to 99.99 mol%, more preferably 99.50 mol% to 99.99 mol%. By using PVA resin with such saponification degree, the effect of improving durability under high temperature and high humidity environment can be suitably obtained.

[0073] The average degree of polymerization of the PVA-based resin can be appropriately selected depending on the intended purpose. The average degree of polymerization is preferably 1,500 to 4,500, more preferably 1,800 to 4,000, and even more preferably 2,000 to 3,500.

[0074] The water-soluble resin concentration (for example, PVA-based resin concentration) in the acidic aqueous solution is preferably 0.02 to 6.0 wt %, more preferably 0.04 to 5.0 wt %, and further preferably 0.1 to 4.0 wt %. With such a resin concentration, a uniform functional film that is closely attached to the polarizing film can be formed.

[0075] The viscosity (20° C.) of the acidic aqueous solution containing the water-soluble resin is preferably 0 mPa·sec to 350 mPa·sec, more preferably 10 mPa·sec to 200 mPa·sec, and further preferably 30 mPa·sec to 120 mPa·sec. Such a viscosity provides good workability (applicability).

[0076] Any appropriate method may be adopted as a coating method of the acidic aqueous solution. Specific examples thereof include the method described in the section A-1-1 as a coating method of a coating liquid for forming a PVA-based resin layer (polarizing film).

[0077] The coating amount of the acidic aqueous solution containing a water-soluble resin can be appropriately set according to the thickness of the functional film as a target. The coating amount of the acidic aqueous solution not containing a water-soluble resin is, for example, 7 g / m 2 ~15g / m 2 , preferably 9g / m 2~11g / m 2 .

[0078] Typically, after the acidic aqueous solution is applied, the coating layer (coated surface) is dried at a drying temperature of, for example, 40° C. to 100° C. and a drying time of, for example, 1 minute to 20 minutes.

[0079] A-2. Method for producing a polarizing plate using a single PVA-based resin film

[0080] In item A-1, a method for manufacturing a polarizing plate using a laminate of a thermoplastic resin substrate and a PVA-based resin layer coated on the thermoplastic resin substrate is described, but the present invention can also be applied to a method for manufacturing a polarizing plate using a single PVA-based resin film. Typically, this manufacturing method includes: stretching and dyeing a self-supporting PVA-based resin film to form a polarizing film with the PVA-based resin film; and coating at least one surface of the polarizing film with an acidic aqueous solution containing an acid component and a pH of 2.5 or less. More specifically, a long strip of PVA-based resin film is uniaxially stretched along the strip direction using a roller stretching machine while being swollen, dyed, cross-linked and cleaned to produce a polarizing film, and an acidic aqueous solution containing an acid component and a pH of 2.5 or less is coated on at least one surface of the polarizing film after the cleaning treatment. The coating of the acidic aqueous solution can be carried out in the same manner as item A-1-7. As needed, a protective layer can be attached to one or both sides of the polarizing film.

[0081] B. Polarizing plate obtained by the manufacturing method of the present invention

[0082] The polarizing plate obtained by the manufacturing method described in item A above includes a polarizing film, and preferably further includes a protective layer provided on at least one side thereof. In the above manufacturing method, when the acidic aqueous solution coated on the surface of the polarizing film contains a water-soluble resin, a polarizing plate having a functional film formed on the coated surface can be obtained.

[0083] Figure 2 It is a method for manufacturing a polarizing plate described in Item A-1, and is a schematic cross-sectional view of an example of a polarizing plate obtained by a manufacturing method using an acidic aqueous solution containing a water-soluble resin. The polarizing plate 10a comprises: a polarizing film 12, a functional film 14 disposed adjacent to one surface of the polarizing film 12, a first protective layer 16 disposed on the side of the polarizing film 12 opposite to the side on which the functional film 14 is disposed, and a second protective layer 18 disposed on the side of the functional film 14 opposite to the side on which the polarizing film 12 is disposed. One of the first protective layer 16 and the second protective layer 18 can be omitted. When one protective layer is omitted, representatively, the protective layer on the functional film side (the second protective layer 18 in the example shown in the figure) can be omitted. It should be noted that the first protective layer 16 can be a thermoplastic resin substrate for making the laminate described in Item A-1-1.

[0084] Figure 3 It is a method for manufacturing a polarizing plate described in Item A-1, and is a schematic cross-sectional view of an example of a polarizing plate obtained by a manufacturing method using an acidic aqueous solution that does not contain a water-soluble resin. The polarizing plate 10b has: a polarizing film 12, a first protective layer 16 arranged on one side of the polarizing film 12, and a second protective layer 18 arranged on the other side of the polarizing film 12. One of the first protective layer 16 and the second protective layer 18 can be omitted. When one protective layer is omitted, representatively, the protective layer on the coating side of the acidic aqueous solution can be omitted. It should be noted that one of the first protective layer and the second protective layer (wherein the protective layer on the side opposite to the coating side of the acidic aqueous solution) can be a thermoplastic resin substrate for making the laminate described in Item A-1-1.

[0085] B-1.Polarizing film

[0086] As described above, the polarizing film is composed of a PVA-based resin film containing iodine. The thickness of the polarizing film is preferably 8 μm or less, more preferably 7 μm or less, further preferably 5 μm or less, and particularly preferably 3 μm or less. The lower limit of the thickness of the polarizing film may be 1 μm in one embodiment and 2 μm in another embodiment. Such a thickness can be achieved, for example, by making a polarizing film using a laminate of a thermoplastic resin substrate and a PVA-based resin layer coated on the thermoplastic resin substrate. When the polarizing film is made of a single PVA-based resin film, the thickness of the polarizing film may be, for example, 12 μm to 35 μm.

[0087] The iodine concentration in the polarizing film is preferably 3% by weight or more, more preferably 4% by weight to 10% by weight, and more preferably 4% by weight to 8% by weight. It should be noted that in this specification, "iodine concentration" refers to the amount of all iodine contained in the polarizing film. More specifically, iodine is present in the polarizing film as I - , I2, I3 - 、PVA / I3 - Complex, PVA / I5 - The iodine concentration in this specification refers to the concentration of iodine in all forms including complexes, etc. The iodine concentration is calculated, for example, from the intensity of fluorescent X-rays by fluorescent X-ray analysis and the thickness of the film (polarizing film).

[0088] The single-piece transmittance of the polarizing film is preferably 42.0% or more, more preferably 42.5% or more, further preferably 43.5% or more, and particularly preferably 45.0% or more. On the other hand, the single-piece transmittance is preferably 48.0% or less, more preferably 46.0% or less. The durability of a thin polarizing film with a high single-piece transmittance in a high temperature and high humidity environment is sometimes reduced, but according to an embodiment of the present invention, even when a thin polarizing film has such a high single-piece transmittance, excellent durability in a high temperature and high humidity environment can be achieved. It should be noted that in this specification, when referred to as single-piece transmittance, orthogonal transmittance and polarization, it refers to the single-piece transmittance, orthogonal transmittance and polarization before the durability test. The polarization of the polarizing film is preferably 98.0% or more, more preferably 99.0% or more. On the other hand, the polarization is preferably 99.998% or less. According to an embodiment of the present invention, it is possible to balance high single-piece transmittance and high polarization degree, and it is possible to achieve excellent durability in a high temperature and high humidity environment as described later. Typically, the single-piece transmittance is a Y value obtained by measuring using an ultraviolet-visible spectrophotometer and performing visibility correction. In addition, the single-piece transmittance is a value when the refractive index of one surface of the polarizing plate is converted to 1.50 and the refractive index of the other surface is converted to 1.53. Typically, the polarization degree is calculated as follows: Based on the parallel transmittance Tp and the orthogonal transmittance Tc measured using an ultraviolet-visible spectrophotometer and corrected for visibility, it is calculated using the following formula.

[0089] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0090] In one embodiment, representatively, the transmittance (single-sheet transmittance) of a thin polarizing film of less than 8 μm is measured as follows: a laminate of a polarizing film (surface refractive index: 1.53) and a protective layer (protective film) (refractive index: 1.50) is used as a measurement object and measured using an ultraviolet-visible spectrophotometer. Depending on the surface refractive index of the polarizing film and / or the refractive index of the surface of the protective layer in contact with the air interface, the reflectivity at the interface of each layer changes, and as a result, the measured value of the transmittance sometimes changes. Therefore, for example, when a protective layer having a refractive index other than 1.50 is used, the measured value of the transmittance can be corrected according to the refractive index of the surface of the protective layer in contact with the air interface. Specifically, the corrected value C of the transmittance uses the reflectivity R1 (transmission axis reflectivity) of polarized light parallel to the transmission axis at the interface between the protective layer and the air layer, and is expressed by the following formula.

[0091] C=R1-R0

[0092] R0=((1.50-1) 2 / (1.50+1) 2 )×(T1 / 100)

[0093] R1=((n1-1) 2 / (n1+1) 2 )×(T1 / 100)

[0094] Here, R0 is the reflectivity of the transmission axis when a protective layer with a refractive index of 1.50 is used, n1 is the refractive index of the protective layer used, and T1 is the transmittance of the polarizing film. For example, when a substrate (cycloolefin film, film with hard coating, etc.) with a surface refractive index of 1.53 is used as a protective layer, the correction amount C becomes about 0.2%. At this time, 0.2% is added to the transmittance obtained by measurement, so that the polarizing film with a surface refractive index of 1.53 can be converted into the transmittance when a protective layer with a refractive index of 1.50 is used. It should be noted that according to the calculation based on the above formula, the change in the correction value C when the transmittance T1 of the polarizing film is changed by 2% is less than 0.03%, and the transmittance of the polarizing film has a limited effect on the value of the correction value C. In addition, when the protective layer has absorption other than surface reflection, appropriate correction can be performed according to the absorption amount.

[0095] In one embodiment, representatively, the change in polarization degree ΔP of the polarizing film after a 240-hour durability test at a temperature of 60° C. and a relative humidity of 95% may be -0.05% or more, preferably -0.04% to 2.00%, and more preferably -0.03% to 1.50%. It should be noted that the change in polarization degree ΔP is represented by the following formula.

[0096] ΔP=P 240 -P0

[0097] (Where P 240 P0 is the degree of polarization after the durability test, and P1 is the degree of polarization before the durability test (the degree of polarization described above).

[0098] B-2. Functional film

[0099] The functional film comprises an acid component and a water-soluble resin. The thickness of the functional film is preferably set to be 0.1 μm or more, more preferably set to be 0.2 μm or more, and further preferably set to be 0.3 μm or more. If the thickness of the functional film is above the above value, the effect of improving the durability in a high temperature and high humidity environment can be suitably obtained. On the other hand, the thickness of the functional film can be set to be 3.0 μm or less.

[0100] B-3. ​​Protective layer

[0101] The first protective layer and the second protective layer are formed by any and appropriate films that can be used as protective layers of polarizing films. As specific examples of materials that become the main components of the film, cellulose resins such as triacetyl cellulose (TAC) can be listed; transparent resins such as polyester, polyvinyl alcohol, polycarbonate, polyamide, polyimide, polyethersulfone, polysulfone, polystyrene, polynorbornene, polyolefin, (meth) acrylic acid, acetate, etc. can be listed. In addition, thermosetting resins or ultraviolet curing resins such as (meth) acrylic acid, urethane, (meth) acrylic acid urethane, epoxy, silicone, etc. can also be listed. In addition, glassy polymers such as siloxane polymers can also be listed. In addition, polymer films recorded in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain can be used, and for example, a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be cited. The polymer film can be, for example, an extrusion molding of the above resin composition.

[0102] Typically, when the polarizing plate 100 is applied to an image display device, the thickness of the protective layer (outer protective layer) disposed on the opposite side of the display panel is 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. It should be noted that when the surface treatment is performed, the thickness of the outer protective layer is the thickness including the thickness of the surface treatment layer.

[0103] When the polarizing plate is applied to an image display device, the thickness of the protective layer (inner protective layer) configured on the display panel side is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and further preferably 10 μm to 60 μm. In one embodiment, the inner protective layer is a phase difference layer having an arbitrary and appropriate phase difference value. At this time, the in-plane phase difference Re (550) of the phase difference layer is, for example, 110 nm to 150 nm. "Re (550)" is the in-plane phase difference measured using light of a wavelength of 550 nm at 23°C, and is calculated using the formula: Re = (nx-ny) × d. Here, "nx" is the refractive index in the direction (i.e., the slow axis direction) when the in-plane refractive index reaches the maximum, "ny" is the refractive index in the direction orthogonal to the slow axis (i.e., the fast axis direction) in the plane, "nz" is the refractive index in the thickness direction, and "d" is the thickness (nm) of the layer (film).

[0104] Example

[0105] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. The measuring methods of various properties are as follows. It should be noted that, unless otherwise specified, the "parts" and "%" in the examples and comparative examples are by weight.

[0106] (1) Thickness

[0107] The polarizing plates of the examples and comparative examples were cut and the cross sections of the polarizing plates were observed using a scanning electron microscope (JSM7100F manufactured by JEOL Ltd.) to measure the thickness of the functional film. The thickness of the polarizing film was measured using an interference film thickness meter (MCPD-3000 manufactured by Otsuka Electronics Co., Ltd.).

[0108] (2) Single-element transmittance, orthogonal transmittance, and polarization

[0109] The single-piece transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc measured for the polarizing plates of the examples and comparative examples (for the single-piece transmittance, for the laminate having the structure of the protective layer / polarizing film before the acidic aqueous solution is applied) using an ultraviolet visible spectrophotometer (LPF200 manufactured by Otsuka Electronics Co., Ltd.) are respectively set as Ts, Tp, and Tc of the polarizing film. These Ts, Tp, and Tc are Y values ​​obtained by measuring using a 2-degree field of view (C light source) of JIS Z8701 and performing visibility correction. The degree of polarization is calculated from the obtained Tp and Tc using the following formula.

[0110] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0111] Next, a glass (alkali-free glass) from which the alkali component has been removed is attached to the acidic aqueous solution coated side of the polarizing plate with the aid of an adhesive, and the plate is placed in an oven set at a temperature of 60°C and a relative humidity of 95% for 240 hours for a durability test. The polarization degree P after the durability test is obtained in the same manner as above. 240 .

[0112] (3) Viscosity

[0113] The viscosity of the acidic aqueous solution was measured using a VISCO METER R85 type viscometer (RE85L manufactured by Toki Sangyo Co., Ltd.) at a measurement temperature of 25° C. and a rotation speed of 0.5 to 100 rpm.

[0114] [Example 1]

[0115] As the thermoplastic resin substrate, a long amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) having a Tg of about 75° C. was used, and one surface of the resin substrate was subjected to a corona treatment.

[0116] 13 parts by weight of potassium iodide was added to 100 parts by weight of a PVA-based resin obtained by mixing polyvinyl alcohol (degree of polymerization: 4200, degree of saponification: 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER") in a ratio of 9:1, and the resulting product was dissolved in water to prepare a PVA aqueous solution (coating liquid).

[0117] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C. to form a PVA-based resin layer having a thickness of 13 μm, thereby producing a laminate.

[0118] The obtained laminate was uniaxially stretched to 2.4 times in the longitudinal direction (length direction) in an oven at 130° C. (in-air auxiliary stretching treatment).

[0119] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).

[0120] Next, the film was immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single-piece transmittance (Ts) of the polarizing plate finally obtained would be 44.0% (dyeing treatment).

[0121] Next, the film was immersed in a crosslinking bath (boric acid aqueous solution obtained by blending 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).

[0122] Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration of 4 wt %, potassium iodide concentration of 5 wt %) at a liquid temperature of 70°C, and was uniaxially stretched (underwater stretching treatment) along the longitudinal direction (length direction) between rollers with different circumferential speeds in such a manner that the total stretching ratio became 5.5 times.

[0123] Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution prepared by mixing 4 parts by weight of potassium iodide with respect to 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment).

[0124] Thereafter, the laminate was dried in an oven maintained at about 90° C. and brought into contact with a SUS heating roll maintained at a surface temperature of about 75° C. (drying shrinkage treatment). The shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment was 2%.

[0125] In this way, a polarizing film with a thickness of 5.0 μm was formed on the resin substrate, and a cycloolefin film (manufactured by ZEON, product name "G-Film") as a protective layer (protective film) was attached to the surface of the polarizing film using a UV curing adhesive (thickness of 1.0 μm). Thereafter, the resin substrate was peeled off to obtain a laminate having a protective layer / polarizing film structure. The single-piece transmittance (Ts) of the obtained laminate was 44.0%. Since the surface refractive index of the polarizing film / protective layer constituting the laminate was 1.53 / 1.53, the single-piece transmittance was a value obtained by correcting the actual measured value by +0.2% and converting it to a state of 1.53 / 1.50.

[0126] Next, an aqueous solution containing hydrogen chloride and not containing a water-soluble resin (aqueous solution containing HCl) was added at 10 g / m 2 The coating amount was applied to the polarizing film surface of the laminate. Then, the coated surface of the aqueous solution containing HCl was dried at 60°C for 5 minutes to obtain a polarizing plate having a protective layer / polarizing film structure in which the acidic aqueous solution was applied to the surface of the side without the protective layer. It should be noted that the pH of the aqueous solution containing HCl was 1.3.

[0127] [Example 2-1]

[0128] As the acidic aqueous solution, an aqueous solution containing hydrogen chloride and polyvinyl alcohol (polymerization degree of 2600, saponification degree of 99.98 mol%) (PVA aqueous solution containing HCl (PVA concentration: 3.5 wt%)) was used, and the PVA aqueous solution containing HCl was applied in a manner such that the thickness of the functional film became 0.4 μm. Except for this, the same operation as in Example 1 was performed to obtain a polarizing plate having a structure of protective layer / polarizing film / functional film. It should be noted that the pH of the PVA aqueous solution containing HCl was 0.9 and the viscosity was 72 mPa·sec.

[0129] [Example 2-2]

[0130] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 2-1 except that a PVA aqueous solution containing HCl was applied so that the thickness of the functional film became 0.8 μm.

[0131] [Example 2-3]

[0132] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 2-1 except that a PVA aqueous solution containing HCl was applied so that the thickness of the functional film became 1.2 μm.

[0133] [Example 3-1]

[0134] As the acidic aqueous solution, an aqueous solution containing sulfuric acid and the above-mentioned polyvinyl alcohol (PVA aqueous solution containing H2SO4 (PVA concentration: 3.5 wt%)) was used, and the PVA aqueous solution containing H2SO4 was applied in a manner such that the thickness of the functional film became 0.6 μm. Except for this, the same operation as in Example 1 was performed to obtain a polarizing plate having a structure of a protective layer / polarizing film / functional film. It should be noted that the pH of the PVA aqueous solution containing H2SO4 was 0.9 and the viscosity was 70 mPa·sec.

[0135] [Example 3-2]

[0136] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 3-1 except that a PVA aqueous solution containing H 2 SO 4 was applied so that the thickness of the functional film became 1.2 μm.

[0137] [Example 4-1]

[0138] As the acidic aqueous solution, an aqueous solution containing hydrogen chloride and the above-mentioned polyvinyl alcohol (PVA aqueous solution containing HCl (PVA concentration: 3.5 wt%)) was used, and the PVA aqueous solution containing HCl was applied so that the thickness of the functional film became 1.2 μm. The same operation as in Example 1 was performed to obtain a polarizing plate having a structure of a protective layer / polarizing film / functional film. It should be noted that the pH of the PVA aqueous solution containing HCl was 0.9 and the viscosity was 70 mPa·sec.

[0139] [Example 4-2]

[0140] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 4-1 except that a PVA aqueous solution containing HCl having a pH of 1.2 was used.

[0141] [Example 4-3]

[0142] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 4-1 except that the PVA aqueous solution containing HCl at pH 1.6 was applied so that the thickness of the functional film became 1.1 μm.

[0143] [Example 4-4]

[0144] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 4-1 except that the PVA aqueous solution containing HCl at pH 1.8 was applied so that the thickness of the functional film became 1.5 μm.

[0145] [Examples 4-5]

[0146] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 4-1 except that the PVA aqueous solution containing HCl at pH 2.0 was applied so that the thickness of the functional film became 1.2 μm.

[0147] [Example 5-1]

[0148] As the acidic aqueous solution, an aqueous solution containing sulfuric acid and the above-mentioned polyvinyl alcohol (PVA aqueous solution containing H2SO4 (PVA concentration: 3.5 wt%)) was used, and the PVA aqueous solution containing H2SO4 was applied in a manner such that the thickness of the functional film became 0.7 μm. Except for this, the same operation as in Example 1 was performed to obtain a polarizing plate having a structure of a protective layer / polarizing film / functional film. It should be noted that the pH of the PVA aqueous solution containing H2SO4 was 1.0 and the viscosity was 70 mPa·sec.

[0149] [Example 5-2]

[0150] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 5-1 except that a PVA aqueous solution containing H 2 SO 4 having a pH of 1.2 was used.

[0151] [Example 5-3]

[0152] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 5-1 except that a PVA aqueous solution containing H 2 SO 4 having a pH of 1.5 was used.

[0153] [Example 5-4]

[0154] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 5-1 except that a PVA aqueous solution containing H 2 SO 4 having a pH of 1.7 was used.

[0155] [Example 5-5]

[0156] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 5-1 except that a PVA aqueous solution containing H 2 SO 4 having a pH of 2.0 was used.

[0157] [Example 6-1]

[0158] As the acidic aqueous solution, an aqueous solution containing nitric acid and the above-mentioned polyvinyl alcohol (PVA aqueous solution containing HNO3 (PVA concentration: 3.5 wt%)) was used, and the PVA aqueous solution containing HNO3 was applied in a manner such that the thickness of the functional film became 0.7 μm. Except for this, the same operation as in Example 1 was performed to obtain a polarizing plate having a structure of protective layer / polarizing film / functional film. It should be noted that the pH of the PVA aqueous solution containing HNO3 was 1.1 and the viscosity was 72 mPa·sec.

[0159] [Example 6-2]

[0160] A polarizing plate having a structure of a protective layer / polarizing film / functional film was obtained in the same manner as in Example 6-1 except that an aqueous solution containing citric acid and the above-mentioned polyvinyl alcohol (PVA aqueous solution containing citric acid (PVA concentration: 3.5 wt%)) was used as the acidic aqueous solution. It should be noted that the pH of the PVA aqueous solution containing citric acid was 1.3 and the viscosity was 75 mPa·sec.

[0161] [Example 6-3]

[0162] A polarizing plate having a structure of a protective layer / polarizing film / functional film was obtained in the same manner as in Example 6-1 except that an aqueous solution containing phosphoric acid and the above-mentioned polyvinyl alcohol (PVA aqueous solution containing phosphoric acid (PVA concentration: 3.5 wt%)) was used as the acidic aqueous solution. It should be noted that the pH of the PVA aqueous solution containing phosphoric acid was 1.1 and the viscosity was 68 mPa·sec.

[0163] [Comparative Example 1]

[0164] A polarizing plate having a structure of protective layer / polarizing film was obtained in the same manner as in Example 1 except that an aqueous solution containing HCl having a pH of 4.0 was used.

[0165] [Comparative Example 2]

[0166] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 4-1 except that a PVA aqueous solution containing HCl having a pH of 3.1 was used.

[0167] [Comparative Example 3]

[0168] A polarizing plate having a structure of protective layer / polarizing film / functional film was obtained in the same manner as in Example 5-1 except that a PVA aqueous solution containing H 2 SO 4 having a pH of 2.6 was used.

[0169] [Reference example]

[0170] A polarizing plate (Ts: 44.0%) having a protective layer / polarizing film structure was obtained in the same manner as in Example 1 except that the acidic aqueous solution was not applied. It should be noted that the polarization degree P0 of the obtained polarizing plate (substantially the polarizing film) before the durability test was 99.8%, which is approximately the same value as the P0 of the polarizing plates of the Examples and Comparative Examples to which the acidic aqueous solution was applied.

[0171] Regarding the polarizing plates (substantially polarizing films) obtained in the above-mentioned examples, comparative examples, and reference examples, ΔP is shown in Table 1. It should be noted that in Table 1, regarding reliability, a value where ΔP is larger than ΔP of the reference example (in other words, the degree of degradation of the optical characteristics based on the durability test is smaller than that of the reference example (including the case where the optical characteristics have been improved)) is recorded as "0", and a value where ΔP is smaller than ΔP of the reference example (in other words, the degree of degradation of the optical characteristics based on the durability test is greater than that of the reference example) is recorded as "×", and the judgment results are shown.

[0172] [Table 1]

[0173]

[0174] As is clear from Table 1, the polarizing plates of Examples of the present invention have excellent durability in a high-temperature and high-humidity environment.

[0175] Industrial Applicability

[0176] The polarizing plate obtained by the production method of the present invention can be suitably used in a liquid crystal display device.

[0177] Description of Reference Numerals

[0178] 10 polarizing plates

[0179] 12 polarizing film

[0180] 14 Functional film

[0181] 16 First protective layer

[0182] 18 Second protective layer

Claims

1. A method for manufacturing a polarizing plate, comprising: An acidic aqueous solution containing an acid component and having a pH of 2.5 or less is applied to at least one surface of the polarizing film, wherein the acidic aqueous solution does not include an acidic aqueous solution containing a water-soluble crosslinking agent of a vinyl alcohol polymer and an acidic aqueous solution containing an oxazoline group-containing polymer. The polarizing film is composed of a polyvinyl alcohol-based resin film containing iodine. The acidic aqueous solution further includes a water-soluble resin, which is coated on at least one surface of the polarizing film and dried to form a functional film.

2. The manufacturing method according to claim 1, wherein: The acid component includes hydrogen chloride.

3. The manufacturing method according to claim 1, wherein: The acid component includes sulfuric acid.

4. The production method according to any one of claims 1 to 3, wherein The water-soluble resin includes a polyvinyl alcohol-based resin.

5. The manufacturing method according to claim 4, wherein: The polymerization degree of the polyvinyl alcohol resin is 1500-4500.

6. The manufacturing method according to claim 4 or 5, wherein: The acidic aqueous solution has a viscosity of 350 mPa·sec or less.

Citation Information

Patent Citations

  • Iodine-containing polarizing film, process for producing the same, and polarizer comprising the same

    CN101137917A

  • Method for manufacturing polarizing film, polarizing sheet and optical laminate

    CN101519502A

  • Polarizing plate comprising polyethylene terephthalate protective film, method for manufacturing same, and image display device and liquid-crystal display device comprising same

    CN106461840A

  • High durable polarizing plate

    JP2008070571A

  • Polarizing plate and optical member

    US20030152718A1