Display screen supporting plate and preparation method thereof, display screen assembly and electronic equipment
By forming a hard chromium or nitriding layer on the titanium alloy or aluminum alloy matrix layer of the display support plate, the problem of difficulty in taking into account weight loss and stiffness in traditional support plates is solved, and rigidity improvement without increasing thickness is achieved. Cost reduction.
Patent Information
- Application Number
- CN202310630061.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-30
AI Technical Summary
Traditional display support plates are difficult to take into account both weight loss and stiffness requirements, and carbon fiber composite materials are costly and non-conductive.
Titanium alloy or aluminum alloy is used as the substrate layer, and a hard chromium or nitriding layer is formed on its support surface to increase the elastic modulus to improve rigidity, taking into account weight reduction and stiffness requirements.
With the unchanged thickness, the rigidity of the display support plate is greatly improved, achieving both weight reduction and rigidity, and reducing production costs.
Smart Images

Figure CN119068761A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic equipment, and in particular to a display screen support plate and a preparation method thereof, a display screen assembly, and electronic equipment. Background Art
[0002] Thinness and lightness is a major trend in the development of electronic devices. How to reduce the weight of electronic devices has attracted the attention of scientific researchers. The support plate is a structure used to support the display screen in the display screen assembly, and it has certain rigidity requirements. Traditional display screen support plates are made of materials such as stainless steel, carbon fiber and its composite materials. However, stainless steel is heavy, which is not conducive to weight reduction of electronic devices. Carbon fiber and its composite materials are lighter, but thicker. In addition, carbon fiber itself is expensive and non-conductive, and requires a conductive coating. Summary of the invention
[0003] Based on this, it is necessary to provide a display screen support plate and a preparation method thereof, a display screen assembly, and an electronic device to solve the problem that the display screen support plate is difficult to take into account both weight reduction requirements and rigidity requirements.
[0004] The first aspect of the present invention is to provide a display screen support plate, the scheme is as follows:
[0005] A display screen support plate comprises a base layer, wherein the base layer comprises a first support surface and a second support surface which are arranged opposite to each other, and at least one of the first support surface and the second support surface is provided with a rigidity enhancement layer;
[0006] The base layer is a titanium alloy layer or an aluminum alloy layer, and the rigidity enhancing layer is a hard chromium layer; or
[0007] The base layer is a titanium alloy layer, and the rigidity enhancing layer is a nitriding layer.
[0008] The second aspect of the present invention is to provide a method for preparing a display screen support plate, the scheme is as follows:
[0009] A method for preparing a display screen support plate comprises the following steps:
[0010] Providing a base layer, wherein the base layer has a first supporting surface and a second supporting surface which are arranged opposite to each other;
[0011] forming a rigidity reinforcement layer on at least one of the first supporting surface and the second supporting surface;
[0012] The base layer is a titanium alloy layer or an aluminum alloy layer, and the rigidity enhancing layer is a hard chromium layer; or
[0013] The base layer is a titanium alloy layer, and the rigidity enhancing layer is a nitriding layer.
[0014] The third aspect of the present invention is to provide a display screen support plate prepared by the above preparation method.
[0015] A fourth aspect of the present invention is to provide a display screen assembly, comprising the display screen support plate and a display module stacked with the display screen support plate.
[0016] A fifth aspect of the present invention is to provide an electronic device, comprising a housing, a circuit board and the display screen assembly, wherein the display screen assembly and the housing form a storage space, and the circuit board is disposed in the storage space.
[0017] Compared with the traditional solution, the display screen support plate and its preparation method, display screen assembly, and electronic device have the following beneficial effects:
[0018] The above-mentioned display screen support plate adopts a titanium alloy layer or an aluminum alloy layer as a base layer. Titanium alloy and aluminum alloy have a relatively low density, and a hard chromium layer is arranged on at least one of the first supporting surface and the second supporting surface relatively arranged with respect to the base layer. The hard chromium layer can greatly improve its elastic modulus. When the titanium alloy layer is used as the base layer, a nitriding layer can also be arranged on at least one supporting surface. By utilizing the high modulus of titanium nitride, the rigidity of the display screen support plate can be greatly improved without changing the thickness, thereby taking into account both the weight reduction requirements and the rigidity requirements.
[0019] The above-mentioned display screen assembly includes the above-mentioned display screen support plate, and thus has corresponding technical characteristics and can obtain corresponding technical effects.
[0020] The above-mentioned electronic device includes the above-mentioned display screen assembly, and thus has corresponding technical features and can obtain corresponding technical effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic structural diagram of a display screen support plate according to Example 1 of the present invention;
[0022] Figure 2 This is a schematic diagram of the structure of a display screen support plate according to Example 2 of the present invention;
[0023] Figure 3 This is a schematic diagram of the structure of the display screen support plate of Example 3 of the present invention;
[0024] Figure 4 This is a schematic diagram of the structure of a display screen support plate according to Example 4 of the present invention;
[0025] Figure 5 A schematic flow chart of a method for preparing a display screen support plate according to an embodiment of the present invention;
[0026] Figure 6 A schematic diagram of a process for obtaining alloy sheets in an example;
[0027] Figure 7 A schematic diagram of a process for pre-treating the surface of an alloy sheet in one example;
[0028] Figure 8 A schematic diagram of a process for etching the surface of an alloy sheet in one example;
[0029] Fig. 9 A schematic diagram of a process for post-processing a hard chrome plated product in one example;
[0030] Fig.10 The present invention is a schematic flow chart of a method for preparing a display screen support plate according to an embodiment of the present invention. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0033] the term
[0034] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0035] In the present invention, "plurality", "multiple", "multiple times", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0036] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of the present invention.
[0037] In the present invention, the words “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0038] In the present invention, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0039] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0040] In the present invention, the first feature being "above" or "below" the second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, the first feature being "above", "above" and "above" the second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. The first feature being "below", "below" and "below" the second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0041] In the present invention, when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may also be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. It should also be understood that when explaining the connection relationship or positional relationship of elements, although not explicitly described, the connection relationship and positional relationship are interpreted as including an error range, which should be within the acceptable deviation range of a specific value determined by those skilled in the art. For example, "approximately", "approximately" or "substantially" may mean within one or more standard deviations, which are not limited here.
[0042] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0043] In the present invention, "electronic equipment" (or simply "terminal") includes but is not limited to a device configured to receive / send communication signals via a wired line connection (such as via a public switched telephone network (PSTN), a digital subscriber line (DSL), a digital cable, a direct cable connection, and / or another data connection / network) and / or via a wireless interface (for example, for a cellular network, a wireless local area network (WLAN), a digital television network such as a DVB-H network, a satellite network, an AM-FM broadcast transmitter, and / or another communication terminal). A communication terminal configured to communicate via a wireless interface may be referred to as a "wireless communication terminal", "wireless terminal" or "mobile terminal". Examples of mobile terminals include, but are not limited to, satellite or cellular phones; personal communication system (PCS) terminals that can combine cellular radiotelephones with data processing, fax and data communication capabilities; PDAs that can include radiotelephones, pagers, Internet / intranet access, web browsers, notepads, calendars and / or global positioning system (GPS) receivers; and conventional laptop and / or palmtop receivers or other electronic devices including radiotelephone transceivers. A mobile phone is an electronic device configured with a cellular communication module.
[0044] The display support plate is a structure used to support the display in the display assembly. At a time when great emphasis is placed on the thinness and lightness of electronic devices such as mobile phones, the display support plate is expected to be both thin and light and have high rigidity.
[0045] Traditional display screen support plates include stainless steel support plates, carbon fiber support plates, and carbon fiber resin composite support plates.
[0046] The elastic modulus of stainless steel is as high as 193GPa, which has good rigidity and low processing cost. However, the density of stainless steel is very high, up to 7.9g / cm 3 If used as a display support plate for a conventional 8-inch folding screen mobile phone, the weight of the display support plate alone is close to 20g, which cannot meet the lightweight requirements and is therefore unacceptable.
[0047] The advantages of carbon fiber include low density and high elastic modulus. The density of carbon fiber is only 1.8g / cm 3 The composite material made by mixing carbon fiber and epoxy resin has a lower density, which can even be lower than 1.6g / cm 3. The modulus of carbon fiber itself is very high in its fiber direction, but the elastic modulus of the composite material of carbon fiber and epoxy resin along the fiber direction is only about 55% of that of carbon fiber, and the elastic modulus of the composite material perpendicular to the fiber direction is basically the elastic modulus of epoxy resin, which is only a few gigapascals and can be basically ignored. In this way, to achieve the same level of rigidity and modulus as stainless steel, the thickness of the composite support plate needs to be greatly increased, which is 50% higher than the thickness of the stainless steel support plate, increasing the thickness of the entire machine. In addition, since carbon fiber and its resin composite materials are not conductive, in order to meet the grounding and shielding requirements of the device, conductive treatment is required on their surface, resulting in high production costs throughout the entire process.
[0048] In order to solve the above problems, the present invention provides a display screen support plate.
[0049] The display screen support plate provided by the present invention comprises a base layer, wherein the base layer comprises a first support surface and a second support surface which are arranged opposite to each other, and at least one of the first support surface and the second support surface is provided with a rigidity enhancement layer.
[0050] The base layer is a titanium alloy layer or an aluminum alloy layer, and the rigidity enhancing layer is a hard chromium layer; or
[0051] The base layer is a titanium alloy layer, and the rigidity enhancing layer is a nitriding layer.
[0052] The above-mentioned display screen support plate adopts a titanium alloy layer or an aluminum alloy layer as a base layer. Titanium alloy and aluminum alloy have a relatively low density, and a hard chromium layer is arranged on at least one of the first supporting surface and the second supporting surface relatively arranged with respect to the base layer. The hard chromium layer can greatly improve its elastic modulus. When the titanium alloy layer is used as the base layer, a nitriding layer can also be arranged on at least one supporting surface. By utilizing the high modulus of titanium nitride, the rigidity of the display screen support plate can be greatly improved without changing the thickness.
[0053] For example, when the thickness of the display support plate is 0.12mm, a hard chromium layer is formed on both sides of the titanium alloy layer, and its elastic modulus is increased from the original 110GPa to more than 150GPa; a hard chromium layer is formed on both sides of the aluminum alloy layer, and its elastic modulus is increased from the original 70GPa to more than 120GPa; a nitriding layer is formed on both sides of the titanium alloy layer, and its elastic modulus is increased from the original 110GPa to more than 170GPa, taking into account both weight reduction requirements and stiffness requirements.
[0054] See also Figure 1 , Figure 1The structure of the display screen support plate 10 of Example 1 is shown. In this example, the display screen support plate 10 includes a base layer 11, a first rigid reinforcement layer 12, and a second rigid reinforcement layer 13. The base layer 11 has a first support surface 111 and a second support surface 112 that are arranged opposite to each other. The first rigid reinforcement layer 12 is arranged on the first support surface 111. The second rigid reinforcement layer 13 is arranged on the second support surface 112.
[0055] In Example 1, a first rigidity reinforcement layer 12 is formed on the first support surface 111 of the base layer 11 by hard chrome plating or nitriding, and the first rigidity reinforcement layer 12 is directly formed on the first support surface 111, that is, the first rigidity reinforcement layer 12 is in direct contact with the first support surface 111. A second rigidity reinforcement layer 13 is formed on the second support surface 112 of the base layer 11 by hard chrome plating or nitriding, and the second rigidity reinforcement layer 13 is directly formed on the second support surface 112, that is, the second rigidity reinforcement layer 13 is in direct contact with the second support surface 112.
[0056] In other examples, the rigidity reinforcement layer may be provided on only one of the supporting surfaces of the base layer.
[0057] For example, see Figure 2 The display screen support plate 20 of Example 2 is shown. In this example, the display screen support plate 20 includes a base layer 21 and a rigid reinforcement layer 22. The base layer 21 has a first support surface 211 and a second support surface 212 that are arranged opposite to each other. The rigid reinforcement layer 22 is arranged on the first support surface 211.
[0058] In Example 2, the rigidity enhancement layer 22 is formed on the first support surface 211 of the base layer 21 by hard chrome plating or nitriding. The rigidity enhancement layer 22 is directly formed on the first support surface 211 , that is, the rigidity enhancement layer 22 is in direct contact with the first support surface 211 .
[0059] If the rigidity enhancement layer is a hard chrome layer, other layers may be arranged between the rigidity enhancement layer and the base layer, that is, the rigidity enhancement layer is indirectly formed on the base layer.
[0060] For example, a connection reinforcement layer may be provided between the rigidity reinforcement layer and the base layer. The connection reinforcement layer may be, for example, but not limited to, a nickel layer. Since the nickel layer has better bonding strength with the hard chrome layer and the base layer, the bonding strength between the hard chrome layer and the base layer may be improved by providing the nickel layer.
[0061] See also Figure 3 , Figure 3The structure of the display screen support plate 30 of Example 3 is shown. The display screen support plate 30 includes a base layer 31, and the base layer 31 has a first support surface 311 and a second support surface 312 that are arranged opposite to each other. A first nickel layer 34 is arranged on the first support surface 311, and a first rigidity enhancement layer 32 is arranged on the side of the first nickel layer 34 away from the first support surface 311. A second nickel layer 35 is arranged on the second support surface 112, and a second rigidity enhancement layer 33 is arranged on the side of the second nickel layer 35 away from the second support surface 312.
[0062] In Example 3, nickel plating is first performed on the two supporting surfaces of the base layer 31 to form a first nickel layer 34 and a second nickel layer 35, respectively, and then the first nickel layer 34 is hard chrome plated to form a first rigidity reinforcement layer 32, and the second nickel layer 35 is hard chrome plated to form a second rigidity reinforcement layer 33. By providing the first nickel layer 34 between the first supporting surface 311 and the first rigidity reinforcement layer 32, and providing the second nickel layer 35 between the second supporting surface 312 and the second rigidity reinforcement layer 33, the bonding force between the first rigidity reinforcement layer 32, the second rigidity reinforcement layer 33 and the base layer 31 can be improved.
[0063] It can be understood that in other examples, the base layer may also be provided with a rigid reinforcement layer directly on one of the support surfaces, and a rigid reinforcement layer indirectly on the other support surface.
[0064] For example, see Figure 4 The display screen support plate 40 of Example 4 is shown. The display screen support plate 40 includes a base layer 41, and the base layer 41 has a first support surface 411 and a second support surface 412 that are arranged opposite to each other. A nickel layer 44 is arranged on the first support surface 411, and a first rigidity enhancement layer 42 is arranged on the side of the nickel layer 44 away from the first support surface 411. A second rigidity enhancement layer 43 is directly arranged on the second support surface 412.
[0065] Optionally, the material of the titanium alloy layer may be, but is not limited to, one or more of TA1 titanium alloy, TA2 titanium alloy, TA3 titanium alloy, TA4 titanium alloy, TC5 titanium alloy, TA7 titanium alloy and TC4 titanium alloy.
[0066] Preferably, the material of the titanium alloy layer is TA4 titanium alloy, which has relatively better ductility and is conducive to making a thin layer structure.
[0067] Optionally, the material of the aluminum alloy layer is selected from one or more of 2 series aluminum alloy, 5 series aluminum alloy, 6 series aluminum alloy and 7 series aluminum alloy.
[0068] Preferably, the material of the aluminum alloy layer is 7 series aluminum alloy.
[0069] In some of these examples, the display support plate has multiple openings, for example, openings in areas where high rigidity is not required, which can reduce weight and reduce stress concentration.
[0070] For example, the display screen support plate includes a first folding area, a bending area and a second folding area, the bending area is located between the first folding area and the second folding area, and the bending area is provided with a plurality of openings, which play a role in reducing the rigidity of the bending area and reducing stress concentration.
[0071] In the area of the openings, the plurality of openings may be arranged in a linear arrangement, an array arrangement, etc. The shape of the openings may be, but is not limited to, one or more of a polygonal shape, a circular shape, an elliptical shape, a long strip shape, and an irregular shape.
[0072] In some of the examples, a plurality of openings are arranged in a matrix, the openings are circular holes with a diameter of 0.1 mm to 0.4 mm, and the distance between the edges of adjacent openings is 0.2 mm to 0.6 mm.
[0073] In some of the examples, multiple openings are arranged in a matrix, the openings are regular hexagonal holes with a side length of 0.1mm to 0.4mm, and the distance between the edges of adjacent openings is 0.2mm to 0.6mm. In some of the examples, the openings are strip holes, multiple openings are arranged in multiple columns, and the openings in adjacent columns are staggered. The width of the opening is 0.08mm to 0.15mm, and the length is, for example, 3mm to 6mm, and the distance between the edges of adjacent openings is 0.15mm to 0.25mm. The above-mentioned openings are opened in the bending zone, and the extension direction of the openings is consistent with the length direction of the bending zone.
[0074] Optionally, the thickness of the display screen support plate may be, but is not limited to, 0.1 mm to 0.17 mm. Under this thickness, the display screen support plate can be better applied to electronic devices such as mobile phones.
[0075] Optionally, the thickness of the base layer may be, but is not limited to, 0.05 mm to 0.12 mm. Preferably, the thickness of the base layer accounts for 40% to 80% of the total thickness of the display support plate, and more preferably 70% to 80%. Under this thickness, the display support plate can maintain a low density and achieve lightweight.
[0076] Optionally, when the rigidity enhancement layer is a hard chrome layer, its thickness may be, but is not limited to, 0.003 mm to 0.02 mm. Further, the total thickness of the rigidity enhancement layer accounts for 2% to 15% of the total thickness of the display screen support plate, and more preferably 10% to 15%. Under this thickness, the rigidity of the display screen support plate can be better improved while maintaining a low density of the display screen support plate.
[0077] In the example where a nickel layer is provided in the display support plate, the thickness of the nickel layer can be, but is not limited to, 0.01 mm to 0.03 mm. Preferably, the thickness of the base layer accounts for 40% to 80% of the total thickness of the display support plate, and more preferably 70% to 80%. The total thickness of the rigid reinforcement layer accounts for 2% to 15% of the total thickness of the display support plate, and more preferably 10% to 15%. The total thickness of the nickel layer accounts for 6% to 20% of the total thickness of the display support plate, and more preferably 10% to 15%. At this thickness, the display support plate has both low density and higher rigidity, and can better improve the bonding force between the rigid reinforcement layer and the base layer.
[0078] Optionally, when the rigidity enhancement layer is a nitriding layer, its thickness is 0.01 mm to 0.05 mm. Furthermore, the total thickness of the rigidity enhancement layer accounts for 2% to 15% of the total thickness of the display screen support plate, and more preferably 10% to 15%. At this thickness, while maintaining a low density of the display screen support plate, the rigidity of the display screen support plate can be better improved. Furthermore, the present invention also provides a method for preparing the display screen support plate of any of the above examples.
[0079] The method for preparing the display screen support plate comprises the following steps:
[0080] Get the base layer;
[0081] A rigidity enhancing layer is formed on at least one of the first supporting surface and the second supporting surface.
[0082] See also Figure 5 A method 50 for preparing a display screen support plate according to an embodiment of the present invention comprises the following steps:
[0083] Step S10, obtaining an alloy sheet, where the alloy sheet is a titanium alloy sheet or an aluminum alloy sheet;
[0084] Step S20, pre-treating the surface of the alloy sheet to obtain a substrate layer;
[0085] Step S30, performing nickel plating on the substrate layer to obtain a nickel-plated product;
[0086] Step S40, performing hard chrome plating on the nickel-plated product to obtain a hard chrome-plated product;
[0087] Step S50, post-processing the hard chrome plated product to obtain a display screen support plate.
[0088] See also Figure 6 In some examples, step S10 specifically includes:
[0089] Step S11, providing an alloy raw material, the alloy raw material is a titanium alloy or an aluminum alloy;
[0090] Step S12, hot rolling the alloy raw material to obtain a hot-rolled sheet;
[0091] Step S13, cold rolling the hot-rolled sheet to obtain a cold-rolled sheet.
[0092] The titanium alloy may be, but is not limited to, one or more of TA1 titanium alloy, TA2 titanium alloy, TA3 titanium alloy, TA4 titanium alloy, TC5 titanium alloy, TA7 titanium alloy and TC4 titanium alloy. Preferably, the titanium alloy is TA4 titanium alloy. The aluminum alloy may be, but is not limited to, one or more of 2 series aluminum alloy, 5 series aluminum alloy, 6 series aluminum alloy and 7 series aluminum alloy. Preferably, the aluminum alloy is 7 series aluminum alloy.
[0093] In some of the examples, the alloy raw material is titanium alloy, and in step S12, the thickness of the hot-rolled sheet obtained by hot rolling is 2 mm to 5 mm, specifically 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, etc. In some of the examples, in step S12, the thickness of the cold-rolled sheet is 0.1 mm to 0.15 mm, specifically 0.1 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, etc.
[0094] In some of the examples, the alloy raw material is an aluminum alloy, and in step S12, the thickness of the hot-rolled sheet obtained by hot rolling is 1 mm to 5 mm, specifically, 1 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, etc. In some of the examples, in step S12, the thickness of the cold-rolled sheet is 0.04 mm to 0.15 mm, specifically, 0.05 mm, 0.1 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, etc.
[0095] In some examples, step S10 may further include:
[0096] Step S14, cutting and slicing the cold-rolled sheet to obtain split sheets.
[0097] The size of the divided sheets is specifically set according to the size of the display screen, for example, a large cold-rolled sheet is divided into a plurality of divided sheets of any size between 1 and 10 inches.
[0098] In some examples, step S10 may further include:
[0099] Step S15, flattening the divided sheets to obtain flattened sheets.
[0100] The flattened sheet has high flatness, which optimizes the product appearance and is also convenient for subsequent pretreatment, electroplating and other processes.
[0101] In some examples, step S10 may further include:
[0102] Step S16, opening a plurality of holes on the flattened sheet to obtain a perforated sheet.
[0103] For example, the alloy sheet includes a first folding area, a bending area and a second folding area, the bending area is located between the first folding area and the second folding area, and the bending area is provided with a plurality of openings, which play a role in reducing the rigidity of the bending area and reducing stress concentration.
[0104] In some examples, a method of creating a plurality of openings includes the following steps:
[0105] Step S161, coating a photoresist layer on the surface of the alloy sheet;
[0106] Step S162, exposing and developing the photoresist layer according to the designed pattern to form an etching opening on the photoresist layer;
[0107] Step S163, etching the surface of the alloy sheet through the etching opening;
[0108] Step S164, removing the remaining photoresist.
[0109] In step S161 , the photoresist layer is baked at a temperature of, for example, 80° C. to 140° C.
[0110] In step S162, a double-sided exposure machine may be used to expose the designed graphic plate, develop the plate in a dedicated developer, and dry the plate at 150°C to 270°C.
[0111] In step S163, the etching is performed by chemical etching, for example. The etching solution used is, for example: an etching solution composed of a certain amount of sulfuric acid, nitric acid, phosphoric acid and other compounds; an etching solution composed of a certain concentration of ammonia solution; an etching solution composed of hydrofluoric acid and hydrochloric acid as oxidants; an aqueous solution composed of hydroiodic acid and boric acid, etc.
[0112] In step S164, a sodium hydroxide aqueous solution with a mass content of 10% can be used for immersion at a temperature of 80°C to 100°C until all the unetched photoresist falls off, and then placed in a dryer for drying at 100°C to 150°C.
[0113] In step S20, the pretreatment performed on the surface of the alloy sheet may be, for example, but not limited to, one or more of sandblasting, etching and activation.
[0114] The surface of the alloy sheet that is pretreated may be only one of the surfaces, or may be multiple surfaces, such as all surfaces. For example, one or more surfaces of the alloy sheet that are to form a rigidity enhancement layer are pretreated. When pretreating different surfaces, the specific treatment methods may be the same or different. The area on which the surface is pretreated may be a partial area on the surface, or may be all areas.
[0115] See also Figure 7 In some examples, step S20 specifically includes:
[0116] Step S21, sandblasting;
[0117] Step S22, etching treatment;
[0118] Step S23, activation treatment.
[0119] In step S21, by sandblasting the surface of the alloy sheet, part of the oxide layer on the surface of the alloy sheet can be removed, thereby improving the bonding strength between the subsequently formed coating and the titanium alloy or aluminum alloy base.
[0120] It can be understood that in other examples, the surface of the alloy sheet may not be subjected to sandblasting, or only sandblasting may be performed as pretreatment.
[0121] In step S22, the surface of the alloy sheet is etched to remove the oxide layer on the surface of the alloy sheet, thereby improving the bonding strength between the subsequently formed coating and the titanium alloy or aluminum alloy base. The alloy sheet is sandblasted and etched in sequence to better remove the oxide layer on the surface of the alloy sheet.
[0122] The etching solution can be a mixture of hydrofluoric acid and nitric acid in a certain concentration and ratio. The titanium alloy is corroded at room temperature until red smoke emerges, and the etching is completed. The surface of the alloy sheet is then cleaned with running water to remove the residual etching agent on the surface.
[0123] It can be understood that in other examples, the surface of the alloy sheet may not be etched, or only the etching process may be performed as pretreatment.
[0124] In step S23, for titanium alloy sheets, the surface of the alloy sheets is activated to form a temporary titanium-fluorine film on the surface of the alloy sheets, which can prevent the alloy sheets from further oxidation, thereby improving the bonding strength between the subsequent coating and the alloy sheets. For aluminum alloy sheets, the surface can be activated with an acid such as dilute nitric acid to remove the oxide film on the surface, thereby improving the bonding strength between the subsequent coating and the alloy sheets.
[0125] It can be understood that in other examples, the surface of the alloy sheet may not be subjected to activation treatment, or only activation treatment may be performed during pretreatment.
[0126] It is understood that in other examples, the pretreatment is not limited to the above-mentioned treatment. In addition, the alloy sheet may not be pretreated.
[0127] In step S30, the base layer is plated with nickel to obtain a nickel-plated product. In step S40, the nickel-plated product is plated with hard chrome to obtain a hard chrome-plated product. Since the bonding strength between the nickel layer, the hard chrome layer and the base layer is better, the bonding strength between the hard chrome layer and the base layer can be improved by providing the nickel layer.
[0128] In some examples, the hard chrome plating process includes the following steps:
[0129] The substrate layer is electrically connected, and its surface on which the hard chrome layer is to be formed is immersed in a chromium-containing electroplating solution for electroplating.
[0130] The chromium-containing electroplating solution may be, for example, a standard chromium plating solution, which includes chromic anhydride with a concentration of 220 g / L to 260 g / L and sulfuric acid with a concentration of 2 g / L to 3 g / L. The concentration of chromic anhydride is, for example, 220 g / L, 230 g / L, 240 g / L, 250 g / L, 260 g / L, etc. The concentration of sulfuric acid is, for example, 2 g / L, 2.2 g / L, 2.4 g / L, 2.6 g / L, 2.8 g / L, 3 g / L, etc.
[0131] During hard chromium plating, the temperature of the chromium-containing electroplating solution is 55°C to 65°C, specifically 55°C, 57°C, 59°C, 61°C, 63°C, and 65°C. The current density is 15A / dm 2 ~30A / dm 2 , for example, 15A / dm 2 、18A / dm 2 、21A / dm 2 、24A / dm 2 、27A / dm 2 、30A / dm 2 The thickness of the coating can be controlled by controlling the electroplating time. Generally, the time for depositing a 1μm coating is about 5min.
[0132] In some of these examples, both supporting surfaces of the base layer are directly hard chrome plated to form a hard chrome layer.
[0133] For example, Figure 1As shown, in Example 1, a first rigid reinforcement layer 12 is formed on the first support surface 111 of the base layer 11 by a hard chrome plating process, and the first rigid reinforcement layer 12 is directly formed on the first support surface 111, that is, the first rigid reinforcement layer 12 is in direct contact with the first support surface 111. A second rigid reinforcement layer 13 is formed on the second support surface 112 of the base layer 11 by a hard chrome plating process, and the second rigid reinforcement layer 13 is directly formed on the second support surface 112, that is, the second rigid reinforcement layer 13 is in direct contact with the second support surface 112.
[0134] In some of these examples, only one of the supporting surfaces of the base layer is hard chrome plated to form a rigidity-enhancing layer.
[0135] For example, Figure 2 As shown, in Example 2, the rigidity enhancement layer 22 is formed on the first support surface 211 of the base layer 21 by a hard chrome plating process. The rigidity enhancement layer 22 is directly formed on the first support surface 211 , that is, the rigidity enhancement layer 22 is in direct contact with the first support surface 211 .
[0136] Before the hard chrome plating, a connection reinforcement layer can be formed on the corresponding support surface, for example, a nickel plating is performed to form a nickel layer, and then a hard chrome plating is performed on the nickel layer to form a rigid reinforcement layer. Since the nickel layer has a better bonding force with the rigid reinforcement layer and the base layer, the bonding force between the rigid reinforcement layer and the base layer can be improved by providing the nickel layer.
[0137] In some of the examples, before forming the first rigidity reinforcement layer, nickel plating is performed on the first support surface to form a first nickel layer, and the first rigidity reinforcement layer is formed on the first nickel layer; before forming the second rigidity reinforcement layer, nickel plating is performed on the second support surface to form a second nickel layer, and the second rigidity reinforcement layer is formed on the second nickel layer.
[0138] For example, Figure 3 As shown, in Example 3, nickel plating is first performed on the two supporting surfaces of the base layer 31 to form a first nickel layer 34 and a second nickel layer 35, respectively, and then a first rigidity enhancement layer 32 is formed on the first nickel layer 34 by a hard chrome plating process, and a second rigidity enhancement layer 33 is formed on the second nickel layer 35 by a hard chrome plating process. That is, the first nickel layer 34 is in direct contact with the corresponding supporting surface of the base layer 31, the first rigidity enhancement layer 32 is in direct contact with the first nickel layer 34, and the second rigidity enhancement layer 33 is in direct contact with the second nickel layer 35.
[0139] In some of these examples, the base layer may also be provided with a rigid reinforcement layer directly on one of the support surfaces and indirectly on the other support surface. Figure 4As shown, in Example 4, nickel plating is performed on the first supporting surface 411 of the base layer 41 to form a nickel layer 44, and then a first rigidity enhancement layer 42 is formed by a hard chrome plating process on the basis of the nickel layer 44. On the second supporting surface 412, a second rigidity enhancement layer 43 is formed directly on the basis of the second supporting surface 412 by a hard chrome plating process.
[0140] In some examples, the rigid reinforcement layer is formed only on one of the first support surface and the second support surface of the base layer. Before forming the rigid reinforcement layer, a nickel plating process is performed on the corresponding support surface to form a nickel layer, and the rigid reinforcement layer is formed on the nickel layer. In these examples, the rigid reinforcement layer is in direct contact with the corresponding support surface of the base layer, and the rigid reinforcement layer is in direct contact with the rigid reinforcement layer.
[0141] It can be understood that in other examples, the base layer may not be subjected to nickel plating.
[0142] See also Fig. 9 In some examples, step S50 specifically includes:
[0143] Step S51, dehydrogenation treatment.
[0144] Step S52, heat treatment.
[0145] In step S51, the hard chrome plated product is subjected to a dehydrogenation treatment to remove hydrogen infiltrated during the electroplating process, thereby preventing hydrogen infiltration from reducing the fatigue strength, mechanical properties and bonding strength of the product.
[0146] It can be understood that in other examples, the hard chrome plated product may not be subjected to dehydrogenation treatment, or only dehydrogenation treatment may be performed as a post-treatment.
[0147] In step S52, by heat treating the hard chrome plated product, nickel atoms in the nickel layer can be diffused into the base layer, thereby improving the bonding strength between the base layer and the plated layer.
[0148] In some of these examples, the heat treatment includes the following steps:
[0149] In a vacuum environment, heat the hard chrome-plated product to 650-850°C and keep it warm for 3-5 hours.
[0150] After the insulation time is over, the hard chrome-plated products are air-cooled with the furnace. Before the furnace temperature drops to 200℃, the vacuum degree of the furnace is maintained. When the furnace temperature drops below 200℃, the vacuum is broken and the parts are taken out.
[0151] It can be understood that in other examples, the hard chrome plated product may not be subjected to heat treatment, or only heat treatment may be performed in the post-treatment.
[0152] It is understood that in other examples, post-processing is not limited to the above-mentioned processing. In addition, post-processing may not be performed on the hard chrome-plated product.
[0153] See also Fig.10 , a method 60 for preparing a display screen support plate according to another embodiment includes the following steps:
[0154] Step S100, obtaining an alloy sheet, wherein the alloy sheet is a titanium alloy sheet;
[0155] Step S200, performing nitriding treatment on the alloy sheet.
[0156] The preparation method of the alloy sheet in step S100 may refer to step S10 in preparation method 50 .
[0157] In step S200 , the nitriding treatment may be, but is not limited to, at least one of a salt bath nitriding treatment, a gas nitriding treatment, and a plasma nitriding treatment.
[0158] In some examples, the steps of the salt bath nitriding process include:
[0159] The workpiece is placed in a salt bath at 700°C to 900°C using cyanide salt for 1h to 3h.
[0160] The cyanide salt is, for example, a mixture of one or more of sodium cyanide, potassium cyanide, etc.
[0161] During the salt bath nitriding process, nitrogen, carbon and a very small amount of oxygen diffuse into the alloy surface to form a diffusion layer strengthened by interstitial atomic solid solution.
[0162] In some examples, the steps of the gas nitriding process include:
[0163] The workpiece is placed in ammonia or nitrogen at normal pressure at 800°C to 1000°C; or the workpiece is placed in ammonia at 1.1MPa to 1.3MPa at 800°C to 1000°C.
[0164] In some examples, the steps of plasma nitriding include:
[0165] The nitrogen-containing gas is decomposed and ionized into nitrogen ions, and the nitrogen ions are bombarded on the surface of the workpiece under the action of the electric field.
[0166] The nitrogen-containing gas is, for example, ammonia, nitrogen, a mixed gas of ammonia and hydrogen, a mixed gas of nitrogen and hydrogen, etc.
[0167] During the plasma nitriding process, the sputtering formed by nitrogen ion bombardment can effectively remove the oxide film on the alloy surface and activate the surface. At the same time, particle bombardment will also form crystal defects on the alloy surface, such as vacancies and dislocations. The above two factors work together to promote the absorption of nitrogen on the alloy surface, thereby increasing the nitriding rate.
[0168] Furthermore, the present invention also provides a display screen assembly, comprising a display screen support plate according to any of the above examples, and also comprising a display module stacked with the display screen support plate.
[0169] The above-mentioned display screen assembly includes the display screen support plate of any of the above-mentioned examples, and thus has corresponding technical features and can obtain corresponding technical effects.
[0170] Furthermore, the present invention also provides an electronic device, comprising a housing, a circuit board and the above-mentioned display screen assembly, wherein the display screen assembly and the housing enclose a containing space, and the circuit board is arranged in the containing space.
[0171] The above-mentioned electronic device includes the above-mentioned display screen assembly, and thus has corresponding technical features and can obtain corresponding technical effects.
[0172] It can be understood that the specific type of the electronic device of the present invention is not particularly limited, and technicians in this field can flexibly choose according to actual conditions. For example, it can be a mobile phone, a smart watch, a PDA or a laptop computer.
[0173] The present invention is further described below in conjunction with specific embodiments and comparative examples, but the present invention is not limited to the following specific embodiments.
[0174] Example 1
[0175] Embodiment 1 provides a display screen support plate and a preparation method thereof, the preparation method comprising the following steps:
[0176] Step S1, preparing a titanium alloy sheet: providing a TA4 titanium alloy raw material, first hot rolling to a thickness of 3 mm, then cold rolling to a thickness of 0.1 mm, cutting, slicing and flattening to obtain a titanium alloy sheet.
[0177] Step S2, pre-treating the surface of the titanium alloy sheet, wherein the pre-treatment includes etching, sandblasting, etching and activation in sequence to obtain a substrate layer.
[0178] Step S3, performing nickel plating on the first supporting surface and the second supporting surface of the base layer to form a first nickel layer and a second nickel layer to obtain a nickel-plated product.
[0179] Step S4, performing hard chrome plating on the first nickel layer and the second nickel layer of the nickel-plated product to form a first rigid reinforcement layer and a second rigid reinforcement layer, thereby obtaining a hard chrome-plated product. The total thickness of the first nickel layer and the first rigid reinforcement layer thereon is 0.01 mm, and the total thickness of the second nickel layer and the second rigid reinforcement layer thereon is 0.01 mm.
[0180] Step S5, post-processing the hard chrome plated product, the post-processing comprising dehydrogenation treatment and heat treatment performed in sequence to obtain a display screen support plate.
[0181] Embodiments 2 to 5
[0182] The preparation methods of the display screen support plates of Examples 2 to 5 are substantially the same as that of Example 1, except that the thicknesses of the substrate layer and the coating layer are different, as shown in Table 1.
[0183] Example 6
[0184] Embodiment 6 provides a display screen support plate and a preparation method thereof, the preparation method comprising the following steps:
[0185] Step S1, preparing aluminum alloy sheets: providing 7 series aluminum alloy raw materials, first hot rolling to a thickness of 3 mm, then cold rolling to a thickness of 0.1 mm, cutting, slicing and flattening to obtain titanium alloy sheets.
[0186] Step S2, pre-treating the surface of the titanium alloy sheet, wherein the pre-treatment includes etching, sandblasting, etching and activation in sequence to obtain a substrate layer.
[0187] Step S3, performing nickel plating on the first supporting surface and the second supporting surface of the base layer to form a first nickel layer and a second nickel layer to obtain a nickel-plated product.
[0188] Step S4, performing hard chrome plating on the first nickel layer and the second nickel layer of the nickel-plated product to form a first rigid reinforcement layer and a second rigid reinforcement layer, thereby obtaining a hard chrome-plated product. The total thickness of the first nickel layer and the first rigid reinforcement layer thereon is 0.01 mm, and the total thickness of the second nickel layer and the second rigid reinforcement layer thereon is 0.01 mm.
[0189] Step S5, post-processing the hard chrome plated product, the post-processing comprising dehydrogenation treatment and heat treatment performed in sequence to obtain a display screen support plate.
[0190] Embodiments 7 to 9
[0191] The preparation methods of the display screen support plates of Examples 7 to 9 are substantially the same as that of Example 6, except that the thicknesses of the substrate layer and the coating layer are different, as shown in Table 1.
[0192] Comparative Example 1
[0193] The display screen support plate provided in Comparative Example 1 is a pure TA4 titanium alloy sheet with a thickness of 0.12 mm.
[0194] Comparative Example 2
[0195] The display screen support plate provided in Comparative Example 2 is a pure 7 series aluminum alloy sheet with a thickness of 0.12 mm.
[0196] The overall density and elastic modulus of the display screen support plates provided in Examples 1 to 9 and Comparative Examples 1 to 2 are shown in Table 1.
[0197] Table 1 Density and elastic modulus of display screen support plates of Examples 1 to 9 and Comparative Examples 1 to 2
[0198]
[0199] Example 10
[0200] Embodiment 10 provides a display screen support plate and a preparation method thereof, the preparation method comprising the following steps:
[0201] Step S1, preparing a titanium alloy sheet: providing a TA4 titanium alloy raw material, first hot rolling to a thickness of 3 mm, then cold rolling to a thickness of 0.1 mm, cutting, slicing and flattening to obtain a titanium alloy sheet.
[0202] Step S2, the titanium alloy sheet is salt-bathed in a mixed salt of sodium cyanide and potassium cyanide at 800°C to form a nitriding layer, thereby obtaining a titanium alloy base layer and a first rigid reinforcement layer and a second rigid reinforcement layer on both sides. The base layer has a thickness of 0.08 mm, and the first rigid reinforcement layer and the second rigid reinforcement layer have a thickness of 0.02 mm.
[0203] Examples 11 to 13
[0204] The preparation methods of the display screen support plates of Examples 11 to 13 are substantially the same as that of Example 10, except that the thicknesses of the base layer and the nitriding layer are different, as shown in Table 2.
[0205] Table 2 Density and elastic modulus of display screen support plates of Examples 10 to 13
[0206]
[0207] Comparative Example 4
[0208] The display screen support plate provided in Comparative Example 4 is a stainless steel plate.
[0209] Comparative Example 5
[0210] The display screen support plate provided in Comparative Example 5 is a carbon fiber plate.
[0211] Comparative Example 6
[0212] The display screen support plate provided in Comparative Example 6 is a titanium alloy / stainless steel composite plate, that is, composite stainless steel sheets are rolled on both sides of the titanium alloy sheet. The thickness of the titanium alloy sheet is 0.086 mm, and the thickness of the stainless steel sheet is 0.022 mm.
[0213] Comparative Example 7
[0214] The display screen support plate provided in Comparative Example 7 is a titanium alloy / copper composite plate, that is, composite copper sheets are rolled on both sides of the titanium alloy sheet. The thickness of the titanium alloy sheet is 0.086 mm, and the thickness of the copper sheet is 0.022 mm.
[0215] The physical parameters and cost evaluation of the display screen support plates provided in Example 5 and Comparative Examples 4 to 7 are shown in Table 3.
[0216] Table 3 Physical parameters and cost evaluation of display screen support plates provided in Example 5 and Comparative Examples 4 to 7
[0217]
[0218] In the cost evaluation, the more “+” signs there are, the higher the cost is. The carbon fiber board itself is relatively expensive and is not conductive, so a conductive layer needs to be provided on it, which is very expensive.
[0219] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0220] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A display screen support plate, characterized in that: A base layer is provided, wherein the base layer has a first supporting surface and a second supporting surface which are arranged opposite to each other, and at least one of the first supporting surface and the second supporting surface is provided with a rigidity reinforcement layer; The base layer is a titanium alloy layer or an aluminum alloy layer, and the rigidity enhancing layer is a hard chromium layer; or The base layer is a titanium alloy layer, and the rigidity enhancing layer is a nitriding layer.
2. The display screen support plate according to claim 1, characterized in that: A first rigidity reinforcement layer is disposed on the first supporting surface, and a second rigidity reinforcement layer is disposed on the second supporting surface of the base layer.
3. The display screen support plate according to claim 2, characterized in that: The first rigidity reinforcement layer is a hard chrome layer, and a first connection reinforcement layer is provided between the first support surface and the first rigidity reinforcement layer; and / or The second rigidity reinforcement layer is a hard chrome layer, and a second connection reinforcement layer is arranged between the second supporting surface and the second rigidity reinforcement layer.
4. The display screen support plate according to claim 3, characterized in that: The first connection enhancing layer is a nickel layer, and the second connection enhancing layer is a nickel layer.
5. The display screen support plate according to claim 1, characterized in that: The overall thickness of the display screen support plate is 0.1 mm to 0.17 mm; The thickness of the titanium alloy layer is 0.05 mm to 0.12 mm, or the thickness of the aluminum alloy layer is 0.04 mm to 0.15 mm.
6. The display screen support plate according to claim 5, characterized in that: The thickness of the hard chromium layer is 0.003 mm to 0.02 mm.
7. The display screen support plate according to claim 5, characterized in that: The thickness of the nitriding layer is 0.01 mm to 0.05 mm.
8. The display screen support plate according to claim 1, characterized in that: The material of the titanium alloy layer is selected from at least one of TA1 titanium alloy, TA2 titanium alloy, TA3 titanium alloy, TA4 titanium alloy, TC5 titanium alloy, TA7 titanium alloy and TC4 titanium alloy; or The material of the aluminum alloy layer is selected from at least one of 2 series aluminum alloy, 5 series aluminum alloy, 6 series aluminum alloy and 7 series aluminum alloy.
9. The display screen support plate according to any one of claims 1 to 8, characterized in that: The display screen support plate is provided with a plurality of openings.
10. A method for preparing a display screen support plate, characterized in that: The following steps are involved: Providing a base layer, wherein the base layer has a first supporting surface and a second supporting surface which are arranged opposite to each other; forming a rigidity reinforcement layer on at least one of the first supporting surface and the second supporting surface; The base layer is a titanium alloy layer or an aluminum alloy layer, and the rigidity enhancing layer is a hard chromium layer; or The base layer is a titanium alloy layer, and the rigidity enhancing layer is a nitriding layer.
11. The method for preparing a display screen support plate according to claim 10, characterized in that: A first rigid reinforcement layer is manufactured on the first supporting surface, and a second rigid reinforcement layer is manufactured on the second supporting surface of the base layer.
12. The method for preparing a display screen support plate according to claim 10 or 11, characterized in that: The first rigidity reinforcement layer is a hard chrome layer, and before forming the first rigidity reinforcement layer, a first connection reinforcement layer is formed on the first support surface, and the first rigidity reinforcement layer is formed on the first connection reinforcement layer; and / or The second rigidity reinforcement layer is a hard chrome layer. Before forming the second rigidity reinforcement layer, a second connection reinforcement layer is formed on the second support surface, and the second rigidity reinforcement layer is formed on the second connection reinforcement layer.
13. The method for preparing a display screen support plate according to claim 10 or 11, characterized in that: The hard chrome layer is formed by hard chrome plating, and the process parameters of the hard chrome plating include: The chromium-containing electroplating solution used contains chromic anhydride with a concentration of 220 g / L to 260 g / L and sulfuric acid with a concentration of 2 g / L to 3 g / L. The temperature of the chromium-containing electroplating solution is 55°C to 65°C, and the current density is 15 A / dm 2 ~30A / dm 2 .
14. The method for preparing a display screen support plate according to claim 10 or 11, characterized in that: The preparation method of the substrate layer comprises the following steps: Obtaining an alloy sheet, wherein the alloy sheet is a titanium alloy sheet or an aluminum alloy sheet; Pre-treating at least one surface of the alloy sheet on which the hard chrome layer is to be formed; The pretreatment includes one or more of sandblasting, etching and activation.
15. The method for preparing a display screen support plate according to claim 14, characterized in that: The pretreatment includes the sandblasting treatment, the etching treatment, and the activation treatment performed in sequence.
16. The method for preparing a display screen support plate according to claim 10 or 11, characterized in that: The method for preparing the display screen support plate further comprises the following steps: Post-processing the display screen support plate having the hard chrome layer formed thereon; The post-treatment includes at least one of a hydrogen removal treatment and a heat treatment.
17. The method for preparing a display screen support plate according to claim 16, characterized in that: The heat treatment comprises the following steps: In a vacuum environment, the display screen support plate is heated to 650° C. to 850° C. and kept warm for 3 h to 5 h.
18. The method for preparing a display screen support plate according to claim 10, characterized in that: The nitriding layer is formed by a nitriding treatment, and the nitriding treatment is selected from at least one of a salt bath nitriding treatment, a gas nitriding treatment, and a plasma nitriding treatment.
19. The method for preparing a display screen support plate according to claim 18, characterized in that: The nitriding treatment satisfies at least one of the following characteristics: (1) The nitriding treatment includes the salt bath nitriding treatment, and the steps of the salt bath nitriding treatment include: The workpiece is subjected to a salt bath at 700°C to 900°C using cyanide salt for 1h to 3h; (2) The nitriding treatment includes the gas nitriding treatment, and the steps of the gas nitriding treatment include: Place the workpiece in ammonia or nitrogen at normal pressure at 800℃~1000℃; or At 800℃~1000℃, place the workpiece in 1.1MPa~1.3MPa ammonia gas; (3) The nitriding treatment includes the plasma nitriding treatment, and the steps of the plasma nitriding treatment include: The nitrogen-containing gas is decomposed and ionized into nitrogen ions, and the nitrogen ions are bombarded on the surface of the workpiece under the action of an electric field.
20. The method for preparing a display screen support plate according to claim 10, characterized in that: A plurality of openings are formed on the base layer.
21. The method for preparing a display screen support plate according to claim 20, characterized in that: The method for opening a plurality of said openings comprises the following steps: Coating a photoresist layer on the surface of the base layer; Exposing and developing the photoresist layer according to a designed pattern to form an etching opening on the photoresist layer; etching the base layer through the etching opening; Remove the remaining photoresist.
22. A display screen assembly, characterized in that: The invention comprises a display module and a display screen support plate as claimed in any one of claims 1 to 9 or a display screen support plate prepared by the preparation method as claimed in any one of claims 10 to 21, wherein the display module is mounted on the display screen support plate.
23. An electronic device, characterized in that: It comprises a shell, a circuit board and the display screen assembly as claimed in claim 22, wherein the display screen assembly and the shell form a receiving space, and the circuit board is arranged in the receiving space.
Citation Information
Patent Citations
Method for enhancing magnet adsorption capacity of stainless steel, supporting device and electronic equipment
CN111748763A
Manufacturing method of flexible titanium metal part capable of being folded and rolled
CN115449861A
Flexible screen supporting piece, flexible screen module and electronic equipment
CN216353073U
Nitriding stainless steel for consumer electronic products
US20100273538A1
Cited By
Exposure, development and etching process system for high-precision under-screen support plate and process method thereof
CN121578602A