Nickel paste as well as preparation method and application thereof

By using a metal oxide cladding of modified ceramic powder in nickel slurry, the problem of mismatch between the nickel electrode and the ceramic dielectric sintering and shrinkage is solved, and the electrical performance of MLCC is significantly improved.

CN119069157APending Publication Date: 2024-12-03GUANGDONG ADVANCED CERAMIC MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411115024.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the sintering and shrinkage of nickel electrodes and ceramic media does not match, resulting in poor electrical performance of MLCC products and limited effects of existing improvement measures.

Method used

Using nickel slurry, including nickel powder, modified ceramic powder, binder and organic solvent, the modified ceramic powder increases the sintering shrinkage temperature through metal oxide coating, matches the sintering shrinkage of nickel slurry and ceramic medium, and reduces sintering shrinkage. Rate.

Benefits of technology

Effectively reduce the sintering shrinkage rate of nickel slurry, improve the electrical performance of MLCC, and improve the stability and performance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993382710000051
    Figure BDA0004993382710000051
  • Figure BDA0004993382710000061
    Figure BDA0004993382710000061
  • Figure BDA0004993382710000062
    Figure BDA0004993382710000062
Patent Text Reader

Abstract

The invention relates to nickel paste and a preparation method and application thereof, and belongs to the technical field of capacitors. The nickel paste comprises nickel powder, modified ceramic powder, a binder and an organic solvent, the weight percentage of the nickel powder in the nickel paste is 40%-60%, and the weight percentage of the modified ceramic powder is 3%-15%; the modified ceramic powder comprises ceramic powder and a coating layer on the surface of the ceramic powder; the coating layer is a metal oxide, and the metal oxide is mainly composed of a metal oxide A, a metal oxide B and magnesium oxide according to the mass ratio of (3.5-5): (1-3): 1; the metal oxide A and the metal oxide B are independently selected from at least one of molybdenum oxide, copper oxide, titanium oxide, cobalt oxide, zirconium oxide, manganese oxide and aluminum oxide, and the metal oxide A is different from the metal oxide B. The sintering shrinkage rate of the nickel paste is low, and the chip multilayer ceramic capacitor can be endowed with excellent electrical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of capacitors, and in particular to a nickel paste and a preparation method and application thereof. Background Art

[0002] Chip multilayer ceramic capacitors (MLCC) are chip capacitors made by stacking and sintering ceramic dielectrics and metal electrodes. They are widely used in consumer electronics, automobiles, home appliances, new energy and other fields due to their advantages of high precision, high integration, low power consumption, large capacity and miniaturization. MLCC consists of ceramic dielectrics, metal inner electrodes and metal outer electrodes. The metal inner electrodes are generally made by printing the inner electrode slurry on the ceramic dielectric layer and then drying and sintering; therefore, the inner electrode slurry plays an important role in MLCC.

[0003] The main components of the internal electrode slurry are metal powder, inorganic powder additives and organic carriers. The metal powder forms a metal network structure through high-temperature sintering to achieve the conductive function. The high content of metal powder in the internal electrode slurry is the main factor affecting the performance of the metal internal electrode. At the same time, since MLCC mostly uses BaTiO3 series ceramics as ceramic media, the sintering temperature is around 1300°C. In order to maintain the continuity of the metal electrode layer after sintering, high-melting-point metal materials are usually selected. For example, early MLCC internal electrode materials mostly used precious metal palladium or palladium-silver alloys. Although the chemical properties of this type of metal powder are stable and can be sintered in the air, it is difficult to achieve large-scale application due to its high price.

[0004] Compared with traditional palladium or palladium-silver alloy, nickel is widely used in MLCC due to its advantages such as good solderability, no ion migration, and low cost. However, when co-sintering MLCC, the sintering shrinkage does not match due to the large difference in the sintering curves of the nickel electrode and the ceramic dielectric, which causes deformation of the electrode layer and the ceramic dielectric layer of the MLCC, and may even further cause sintering cracking or peeling. At present, the existing technology mainly increases the sintering shrinkage starting temperature of the internal electrode by coating the surface of the nickel powder or adding specific oxides and compound powders, but the improvement effect is limited, and it is difficult to effectively reduce the sintering shrinkage rate of the internal electrode, which leads to poor electrical performance of the product. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a nickel slurry and a preparation method and application thereof.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] In a first aspect, the present invention provides a nickel paste, which comprises nickel powder, modified ceramic powder, a binder and an organic solvent; the weight percentage of the nickel powder in the nickel paste is 40% to 60%, and the weight percentage of the modified ceramic powder is 3% to 15%;

[0008] The modified ceramic powder includes ceramic powder and a coating layer on the surface of the ceramic powder;

[0009] The coating layer is a metal oxide, and the metal oxide is mainly composed of metal oxide A, metal oxide B and magnesium oxide in a mass ratio of (3.5-5):(1-3):1;

[0010] The metal oxide A and the metal oxide B are independently selected from at least one of molybdenum oxide, copper oxide, titanium oxide, cobalt oxide, zirconium oxide, manganese oxide and aluminum oxide, and the metal oxide A is different from the metal oxide B.

[0011] The present invention combines specific metal oxide A and metal oxide B with magnesium oxide to form a metal oxide coating layer on the surface of a ceramic powder core to obtain a modified ceramic powder. This is not only beneficial for the modified ceramic powder to be evenly distributed around the nickel powder and coated on the surface of the nickel powder during the slurrying process, but also enables the modified ceramic powder to utilize the interaction between the metal oxide coating layer and the ceramic powder core during the sintering process to increase the initial sintering shrinkage temperature of the nickel slurry, so that the sintering shrinkage of the nickel slurry matches the sintering shrinkage of the ceramic medium, and reduces the sintering shrinkage rate of the nickel slurry, thereby effectively improving the electrical properties of the product.

[0012] The content of modified ceramic powder in nickel paste plays a key role. When the weight percentage of modified ceramic powder is too large, it will cause the nickel paste to agglomerate during the sintering process; when the weight percentage of modified ceramic powder is too small, it is difficult to effectively reduce the sintering shrinkage of nickel paste.

[0013] The coating layer on the surface of the ceramic powder refers to a layer structure formed by the metal oxide coating the surface of the ceramic powder in a scattered manner, or a layer structure formed by coating the surface of the ceramic powder in a partially continuous manner, or a layer structure formed by coating the surface of the ceramic powder in a completely continuous manner (i.e., complete coating). In addition, metal oxide A is different from metal oxide B, which means that at least one metal oxide in metal oxide A is different from the metal oxide in metal oxide B.

[0014] Optionally, in terms of mass fractions, when the magnesium oxide in the above-mentioned metal oxide is 1 part, the metal oxide A can specifically be 3.6 parts, 3.8 parts, 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, or 4.8 parts; the metal oxide B can specifically be 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, or 2.8 parts.

[0015] As a preferred embodiment of the nickel paste of the present invention, the weight percentage of the binder in the nickel paste is 2% to 6%, and the weight percentage of the organic solvent is 35% to 55%.

[0016] Optionally, the weight percentage of nickel powder in the above-mentioned nickel paste can be 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58%; the weight percentage of modified ceramic powder can be 4%, 6%, 8%, 10%, 12%, 14%; the weight percentage of binder can be 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%; the weight percentage of organic solvent can be 36%, 38%, 40%, 42%, 44%, 46%, 48%, 50%, 52%, 54%.

[0017] As a preferred embodiment of the nickel paste of the present invention, the nickel paste comprises the following components by weight percentage: 45% to 55% nickel powder, 5% to 10% modified ceramic powder, 3% to 5% binder, and 39% to 50% organic solvent. More preferably, the nickel paste comprises the following components by weight percentage: 50% nickel powder, 7% modified ceramic powder, 4% binder, and 39% organic solvent.

[0018] As a preferred embodiment of the nickel paste of the present invention, the metal oxide A is at least one of molybdenum oxide and titanium oxide; and / or the metal oxide B is at least one of copper oxide and cobalt oxide.

[0019] As a preferred embodiment of the nickel paste of the present invention, the modified ceramic powder is obtained by mixing ceramic powder and metal oxide and then subjecting the mixture to low temperature heat treatment, wherein the temperature of the low temperature heat treatment is 300-600° C. and the time is 1-5 hours.

[0020] Optionally, the atmosphere of the low-temperature heat treatment is air; the temperature of the low-temperature heat treatment can be specifically 350°C, 400°C, 450°C, 500°C, 550°C, and the time of the low-temperature heat treatment can be specifically 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h.

[0021] As a preferred embodiment of the nickel paste of the present invention, the mass ratio of the ceramic powder to the metal oxide is 100:0.5 to 100:2. Optionally, the mass ratio of the ceramic powder to the metal oxide can be 100:0.6, 100:0.8, 100:1, 100:1.2, 100:1.4, 100:1.6, 100:1.8. Among them, the amount of metal oxide added relative to the ceramic powder has an important influence on the shrinkage effect of the nickel paste and the electrical properties of the product. Studies have found that when the mass ratio of ceramic powder to metal oxide is in the range of 100:(0.5 to 2), it can not only effectively prevent the metal oxide from entering the dielectric layer of the product during the product sintering process to better maintain the electrical properties of the product, but also give the nickel paste a better shrinkage delay effect.

[0022] As a preferred embodiment of the nickel paste of the present invention, the D50 particle size of the ceramic powder is smaller than the D50 particle size of the nickel powder; more preferably, the D50 particle size of the ceramic powder is ≤100nm, and / or, the D50 particle size of the nickel powder is ≥120nm; further preferably, the D50 particle size of the ceramic powder is 10-100nm, and / or, the D50 particle size of the nickel powder is 120-400nm.

[0023] Optionally, the D50 particle size of the ceramic powder may be 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, or 90 nm, and the D50 particle size of the nickel powder may be 150 nm, 200 nm, 250 nm, 300 nm, or 350 nm.

[0024] The D50 particle size of the ceramic powder or nickel powder can be obtained by taking pictures of the ceramic powder or nickel powder under a field emission electron microscope and counting the particle sizes. In addition, the ceramic powder or nickel powder can be made by yourself or purchased.

[0025] As a preferred embodiment of the nickel paste of the present invention, the ceramic powder is at least one of barium titanate, barium calcium titanate, and barium strontium titanate.

[0026] As a preferred embodiment of the nickel paste of the present invention, the binder is at least one of ethyl cellulose, epoxy resin, phenolic resin, rosin, and polyvinyl butyral.

[0027] As a preferred embodiment of the nickel paste of the present invention, the organic solvent is at least one of octanol, terpineol, dibutyl phthalate and diethyl phthalate.

[0028] In a second aspect, the present invention provides a method for preparing the above nickel paste, which comprises the following steps: uniformly mixing nickel powder, modified ceramic powder, a binder and an organic solvent to obtain the nickel paste.

[0029] In a third aspect, the present invention provides the use of the above nickel paste in the preparation of chip-type multilayer ceramic capacitors.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention combines specific metal oxide A and metal oxide B with magnesium oxide to form a metal oxide coating layer on the surface of the ceramic powder, which is not only conducive to the uniform distribution of the modified ceramic powder around the nickel powder and coating on the surface of the nickel powder during the slurrying process, but also enables the modified ceramic powder to utilize the interaction between the metal oxide coating layer and the ceramic powder core during the sintering process to increase the initial sintering shrinkage temperature of the nickel slurry, so that the sintering shrinkage of the nickel slurry matches the sintering shrinkage of the ceramic medium, and reduces the sintering shrinkage rate of the nickel slurry, thereby effectively improving the electrical properties of the product. DETAILED DESCRIPTION

[0032] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0033] Unless otherwise specified, other materials, reagents, etc. used in the examples and comparative examples can be obtained from commercial sources.

[0034] 1. Raw materials and reagents

[0035] Nickel powder, D50 particle size 300nm, commercially available;

[0036] The ceramic powder is barium calcium titanate, with a D50 particle size of 80 nm, commercially available;

[0037] The binder is prepared by compounding ethyl cellulose and polyvinyl butyral in a weight ratio of 1:3, wherein the ethyl cellulose and polyvinyl butyral are both commercially available;

[0038] The organic solvent is prepared by compounding terpineol and diethyl phthalate in a weight ratio of 1:1, wherein the terpineol and diethyl phthalate are both commercially available.

[0039] 2. Modified ceramic powder

[0040] Table 1 Mass fraction of each component in modified ceramic powders 1 to 27

[0041]

[0042]

[0043] The method for preparing the modified ceramic powder comprises the following steps:

[0044] The metal oxide was ground and dispersed by a sand mill (grinding rate was 1000 r / min, grinding time was 1 h), and then the ground metal oxide and ceramic powder were mixed according to a ratio (grinding rate was 3000 r / min, grinding time was 1 h), and then low-temperature heat treatment was carried out in an air atmosphere at 300°C for 5 h to obtain the modified ceramic powder.

[0045] 3. The preparation method of nickel paste of the present invention comprises the following steps:

[0046] The modified ceramic powder is mixed evenly with nickel powder, a binder and part of the organic solvent (grinded and mixed by a sand mill at a grinding rate of 1000 r / min and a grinding time of 3 h), and then rolled (rolled by a three-roll mill with a rolling pressure controlled at 15 to 30 N / mm). After passing the rolling test, the remaining organic solvent is added for dilution and filtered (filtered with a 2 μm filter element) to obtain the nickel slurry.

[0047] 4. Performance Testing

[0048] (1) Viscosity

[0049] The test method is: using a viscometer to measure the viscosity of the nickel slurry at 25°C and a rotation speed of 10r / min.

[0050] (2) Solid content

[0051] The test method is: nickel paste (about 2-4g) is evenly coated on an empty substrate plate, then transferred to a drying oven to dry the solvent, and then the solid content (SC%) of the nickel paste is calculated according to the following formula;

[0052]

[0053] In the above formula, G1 is the mass of the empty substrate plate, G2 is the total mass of the empty substrate plate + the nickel paste after coating with nickel paste and before drying, and G3 is the total mass of the empty substrate plate + the nickel paste after drying.

[0054] (3) Shrinkage

[0055] Test method: Place the nickel slurry in a crucible, dry it in a belt drying furnace, and then remove the glue in a special MLCC debinding box. After sieving with 200 mesh, grind the sieved powder and camphor oil evenly at a mass ratio of 100:5, and press it into a cylindrical sample (bottom diameter of 5 cm and height of 8 cm) at 100MPa through upper and lower pressure head molds; then use a thermomechanical analyzer (TMA) to test (test conditions: atmosphere is 98% by volume N2 + 2% by volume H2, temperature range is 200-1200°C, heating rate is 10K / min) The volume change of the cylinder is calculated, and the shrinkage rate (α%) of the cylindrical sample is calculated according to the following formula;

[0056]

[0057] V0 in the above formula is the volume of the cylindrical sample before sintering (i.e., the volume before TMA test), cm 3 ; V1 is the volume of the cylindrical sample after sintering, cm 3 (i.e. the volume after TMA test).

[0058] (4) Electrical properties

[0059] Test method: Use the nickel paste in each embodiment and comparative example as the conductive paste for internal electrodes, respectively, to make 100 multilayer ceramic capacitors (MLCCs) each, and then conduct voltage test at 150°C and 80V for 12h (100 MLCCs tested), and calculate the average failure time of MLCC (average failure time = total failure time of 100 MLCCs / 100); the failed part is calculated according to the actual failure time, and the non-failed part is calculated according to the 12h failure.

[0060] The preparation method of the above-mentioned MLCC is: coating a nickel electrode slurry (i.e., the nickel slurry in each embodiment and comparative example) on a ceramic dielectric layer, drying, and forming an inner electrode layer on the ceramic dielectric layer; then stacking to obtain a capacitor substrate; and finally, respectively arranging a first terminal electrode and a second terminal electrode at both ends of the capacitor substrate to obtain an MLCC.

[0061] Examples 1 to 22 and Comparative Examples 1 to 11

[0062] The formula and properties of the nickel pastes in Examples 1 to 7 and Comparative Examples 1 to 4 are shown in Table 1, wherein the modified ceramic powders are all modified ceramic powder 1.

[0063] Table 1 Formula and performance of nickel paste in Examples 1 to 7 and Comparative Examples 1 to 4

[0064]

[0065]

[0066] The nickel paste in Examples 8 to 22 is basically the same as that in Example 1 (i.e., in terms of weight percentage, the nickel paste in Examples 8 to 22 includes 50% nickel powder, 7% modified ceramic powder, 4% binder and 39% organic solvent), the difference being that the components of the modified ceramic powder are different, as specifically shown in Table 2.

[0067] The nickel paste in Comparative Examples 5 to 16 is basically the same as that in Example 1 (i.e., in terms of weight percentage, the nickel paste in Comparative Examples 5 to 16 includes 50% nickel powder, 7% modified ceramic powder (or ceramic powder), 4% binder and 39% organic solvent), the difference being that the components of the modified ceramic powder are different, as specifically shown in Table 2.

[0068] Table 2 Formulation and performance of nickel paste in Examples 8 to 22 and Comparative Examples 5 to 16

[0069]

[0070]

[0071] According to the data in Table 1 and Table 2, the shrinkage rate of the nickel paste in Examples 1 to 22 is less than or equal to 5.8%, and the electrical properties of the corresponding ceramic capacitors (average failure time of the product) are all above 6.3h, indicating that the nickel paste of the present invention has a low sintering shrinkage rate and can significantly improve the electrical properties of the ceramic capacitor.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A nickel paste, characterized in that: The nickel slurry comprises nickel powder, modified ceramic powder, a binder and an organic solvent; the weight percentage of the nickel powder in the nickel slurry is 40% to 60%, and the weight percentage of the modified ceramic powder is 3% to 15%; The modified ceramic powder includes ceramic powder and a coating layer on the surface of the ceramic powder; The coating layer is a metal oxide, and the metal oxide is mainly composed of metal oxide A, metal oxide B and magnesium oxide in a mass ratio of (3.5-5):(1-3):1; The metal oxide A and the metal oxide B are independently selected from at least one of molybdenum oxide, copper oxide, titanium oxide, cobalt oxide, zirconium oxide, manganese oxide and aluminum oxide, and the metal oxide A is different from the metal oxide B.

2. The nickel paste according to claim 1, characterized in that The weight percentage of the binder in the nickel paste is 2% to 6%, and the weight percentage of the organic solvent is 35% to 55%.

3. The nickel paste according to claim 1, characterized in that The metal oxide A is at least one of molybdenum oxide and titanium oxide; And / or, the metal oxide B is at least one of copper oxide and cobalt oxide.

4. The nickel paste according to claim 1, characterized in that The modified ceramic powder is obtained by mixing ceramic powder and metal oxide and then subjecting the mixture to low temperature heat treatment, wherein the temperature of the low temperature heat treatment is 300-600° C. and the time is 1-5 hours.

5. The nickel paste according to claim 4, characterized in that The mass ratio of the ceramic powder to the metal oxide is 100:0.5 to 100:

2.

6. The nickel paste according to claim 1, characterized in that The D50 particle size of the ceramic powder is smaller than the D50 particle size of the nickel powder.

7. The nickel paste according to claim 6, characterized in that The D50 particle size of the ceramic powder is 10 to 100 nm; and / or the D50 particle size of the nickel powder is 120 to 400 nm.

8. The nickel paste according to any one of claims 1 to 7, characterized in that At least one of the following (I) to (III): (I) The ceramic powder is at least one of barium titanate, barium calcium titanate, and barium strontium titanate; (II) the binder is at least one of ethyl cellulose, epoxy resin, phenolic resin, rosin, and polyvinyl butyral; (III) The organic solvent is at least one of octanol, terpineol, dibutyl phthalate and diethyl phthalate.

9. The method for preparing nickel paste according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: uniformly mixing nickel powder, modified ceramic powder, a binder and an organic solvent to obtain nickel slurry.

10. Use of the nickel paste according to any one of claims 1 to 8 in the preparation of chip-type multilayer ceramic capacitors.

Citation Information

Cited By

  • Regulation and control method for matching sintering shrinkage of MLCC electrode nickel paste with BaTiO3 ceramic medium

    CN122444545A