Electrostatic chuck and method for repeatedly using electrostatic chuck

By growing the film on the contact layer of the electrostatic suction cup and removing the pollution by acid etching, the adsorption problem caused by ceramic layer pollution is solved, and the reusable use and service life of the electrostatic suction cup is achieved.

CN119069412APending Publication Date: 2024-12-03AISINA SEMICON TECH (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411303613.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

After the ceramic layer is contaminated or eroded during use of the existing electrostatic suction cup, the existing cleaning and polishing methods will damage the surface plane and roughness, resulting in adsorption unevenness and plasma etching unevenness, thereby reducing performance and resulting in scrapping.

Method used

One or more films are evenly grown on the contact layer of the electrostatic suction cup, and the contaminated film is removed by using the high etching rate difference of the acid etchant without damaging the contact layer, and then the new film is re-plating to extend the service life.

Benefits of technology

After the contaminated film is removed by acid etching, the contact layer of the electrostatic suction cup can be re-coated, extending the service life of the equipment and maintaining adsorption performance, avoiding scrapping problems caused by uneven adsorption force.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069412A_ABST
    Figure CN119069412A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrostatic chucks, in particular to an electrostatic chuck and a reusable method of the electrostatic chuck. The electrostatic chuck includes: a substrate; the electrode layer, the contact layer and the thin film are sequentially stacked on the substrate; the etching rate of the acid etching etchant to the thin film is greater than the etching rate of the acid etching etchant to the contact layer. According to the invention, one or more layers of films are uniformly grown on the contact layer of the electrostatic chuck by applying an additive manufacturing method, the polluted films can be selectively removed after the electrostatic chuck is used, and because the etching rate of the etching agent for acid etching to the films is greater than the etching rate of the etching agent for acid etching to the contact layer, the film can be removed from the contact layer. The thin film can be removed in an acid etching mode without damaging the contact layer, and a new thin film can be plated again after the thin film is removed, so that the service life of the electrostatic chuck is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrostatic chucks, and in particular to an electrostatic chuck and a method for reusing the electrostatic chuck. Background Art

[0002] The ceramic surface of the existing electrostatic chuck may be contaminated or eroded by process products during use, resulting in deformation of the ceramic layer. At present, cleaning and polishing methods are generally used to treat the contaminated or eroded ceramic layer to extend the life of the electrostatic chuck. However, this method will affect the flatness and roughness of the surface, and the number of cleaning and polishing is limited, which is an irreversible damage.

[0003] During the long-term use of cleaning and polishing of the surface, changes in morphology, flatness, uniformity, etc. will affect the adsorption and adsorption uniformity of the electrostatic chuck, which will lead to uneven plasma etching on the surface of the electrostatic chuck, a significant decrease in yield, and even silicon wafer breakage due to uneven adsorption force, resulting in overall scrapping.

[0004] Currently, after the performance of the electrostatic chuck deteriorates due to multiple cleaning and polishing, the only option is to scrap or remove the original ceramic layer and adhere a new ceramic layer. Summary of the invention

[0005] The electrostatic chuck is a core component in the semiconductor manufacturing process. Whenever the ceramic layer is contaminated or corroded, the existing treatment method is to remove the entire ceramic layer on the surface of the electrostatic chuck and then re-gluing a new ceramic layer. The ceramic layer on the electrostatic chuck is precisely constructed, with not only a complex and delicate morphology on the surface, but also a metal electrode layer built into the inner layer. Removing and re-gluing a new ceramic layer each time is not only expensive but also time-consuming and labor-intensive. In order to solve at least one of the above-mentioned shortcomings of the existing electrostatic chuck, the present invention provides an electrostatic chuck and a method for reusing the electrostatic chuck.

[0006] In order to solve the above technical problems, one of the technical solutions provided by the present invention is as follows: An electrostatic chuck, comprising: substrate; and An electrode layer, a contact layer and a thin film are sequentially stacked on the substrate; The etching rate of the thin film by the acid etching etchant is greater than the etching rate of the contact layer by the acid etching etchant.

[0007] The present invention proposes to use additive manufacturing to uniformly grow one or more thin films on the contact layer of the electrostatic chuck. After the electrostatic chuck is used, the contaminated film can be removed. Due to the difference in etching rates between the formed contact layer and the film, the film can be removed by acid etching without damaging the contact layer. After removal, a new film can be re-plated, thereby extending the service life of the electrostatic chuck.

[0008] In one embodiment, the ratio of the etching rate of the thin film by the acid etching etchant to the etching rate of the contact layer by the acid etching etchant is greater than 100:1; the larger etching rate difference of the acid etching is utilized to make it easier to clean the thin film on the contact layer with less impact on the contact layer.

[0009] In one embodiment, the material of the film is an oxide material that is easily corroded by acid and resistant to plasma corrosion. In order to make it easier to remove the used film and form a new film, it is more appropriate to select an oxide material that is easily corroded by acid and resistant to plasma corrosion.

[0010] Preferably, the material of the film is selected from a group consisting of a metal compound of group IIIB, a metal compound of group IVB, a metal compound of group IIIA, a non-metal compound of group IVA, or a combination of the above compounds; Preferably, the material of the film is selected from yttrium oxide, aluminum oxide, aluminum nitride, silicon oxide, silicon nitride, titanium nitride, diamond-like carbon, or a composite material thereof.

[0011] In one embodiment, the thickness of the film is greater than 0.5 μm and less than 50.0 μm. The film should not be too thick, which will easily affect its adhesion to the contact layer and make the electrostatic adsorption force worse, while too thin will make it difficult to play the role required for setting the film.

[0012] In one embodiment, the contact layer is an insulating layer, and the thin film is made of an insulating oxide material; or the contact layer is a conductive layer, and the thin film is made of a conductive oxide material.

[0013] In one embodiment, the ratio of the resistivity of the film to the resistivity of the contact layer is less than or equal to 5:1; since the electrostatic chuck needs to apply voltage to implement adsorption, if the resistivity of the intermediate film is too high or low, it will affect the adsorption performance. Preferably, the resistivity of the contact layer and the film layer should be at the same order of magnitude. Therefore, the present application has found through experiments that the resistivity of the two is 5:1 or less, which can fully meet the adsorption effect required by the electrostatic chuck; Preferably, the ratio of the resistivity of the film to the resistivity of the contact layer is 1:1.

[0014] In one embodiment, the contact layer is formed by sintering, and the thin film is formed by vacuum coating. The present invention prepares the contact layer and the thin film by sintering and vacuum coating respectively, so that the etching rate of the thin film by the acid etching etchant is greater than the etching rate of the contact layer by the acid etching etchant.

[0015] In one embodiment, the film is a multi-layer film structure, and the multi-layer film structure includes a bottom film close to the contact layer and a surface film away from the contact layer; the porosity of the bottom film is greater than that of the surface film; When the film is a multi-layer film structure, the porosity of the bottom film is greater than that of the surface film, thereby playing a role in stress release, improving the adhesion of the surface film, and making it less likely to peel off under the expansion stress of high and low temperature differences; the surface film has a small porosity and is therefore denser, better in corrosion resistance, and can play a better protective role.

[0016] Preferably, the porosity of the bottom film is greater than 1.0‰ and less than 5.0‰, and the porosity of the surface film is less than 0.1‰; Preferably, the material of the bottom film is aluminum oxide, and the material of the surface film is yttrium oxide.

[0017] The second technical solution provided by the present invention is as follows: The present invention provides a method for reusing the electrostatic chuck as described above, the method comprising the following steps: forming a patterned mask to protect the portion of the electrostatic chuck susceptible to chemical corrosion and to expose the contact layer and the thin film; performing acid etching on the contact layer and the thin film to remove the thin film; cleaning and drying the electrostatic chuck after removing the film; A thin film is formed on the contact layer.

[0018] In one embodiment, the acid etching includes immersion, spraying, or horizontal rinsing, wherein the etchant used for the acid etching is selected from hydrofluoric acid and / or nitric acid.

[0019] In one embodiment, the acid etching rate of the thin film is greater than the acid etching rate of the contact layer.

[0020] Based on the above, compared with the prior art, the electrostatic chuck provided by the present invention includes at least one of the following beneficial technical effects: The electrostatic chuck provided by the present invention uniformly grows one or more layers of thin film on the contact layer, and the thin film has good compactness and can physically separate the polymer and pollutants generated in the process from the original contact layer of the electrostatic chuck; the thin film has good adhesion and will not fall off during the service life; the thin film can be prepared by using ceramic materials such as yttrium oxide, aluminum oxide, aluminum nitride, etc., and has the characteristic of anti-plasma etching; the etching rate of the thin film by the acid etching etchant is greater than the etching rate of the contact layer by the acid etching etchant, so the contact layer of the original electrostatic chuck will not be affected in the process of removing the thin film; after the thin film is removed from the electrostatic chuck provided by the present invention, a thin film can be plated again on the contact layer of the electrostatic chuck to achieve the purpose of repeated cleaning and utilization, thereby extending the service life of the electrostatic chuck.

[0021] Other features and beneficial effects of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other beneficial effects of the present invention can be realized and obtained by the structures particularly pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. The positional relationships described in the drawings in the following description are based on the directions in which the components are drawn in the diagrams, unless otherwise specified.

[0023] Figure 1-Figure 4 A schematic diagram of a manufacturing method of an electrostatic chuck provided by the present invention; Figure 5 A schematic diagram of the structure of an electrostatic chuck provided by an embodiment of the present invention; Figure 6 The present invention is a flowchart of a method for reusing an electrostatic chuck.

[0024] Reference numerals: 1. Electrostatic chuck; 10. Substrate; 10a. Upper surface; 10b. Lower surface; 20. Electrode layer; 20a. Top surface; 20b. Side surface; 30. Contact layer; 40. Film; 41. Bottom film; 42. Surface film. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; the technical features designed in different implementation modes of the present invention described below can be combined with each other as long as they do not conflict with each other; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] In the description of the present invention, it should be noted that all terms (including technical terms and scientific terms) used in the present invention have the same meanings as those generally understood by ordinary technicians in the field to which the present invention belongs, and should not be understood as limitations on the present invention; it should be further understood that the terms used in the present invention should be understood to have the same meanings as these terms in the context of this specification and in the relevant fields, and should not be understood in an idealized or overly formal sense, unless explicitly defined in this invention.

[0027] An embodiment of the present invention provides an electrostatic chuck, the electrostatic chuck 1 comprising: a substrate 10; and An electrode layer 20, a contact layer 30 and a thin film 40 are sequentially stacked on the substrate 10; The etching rate of the thin film 40 by the acid etching etchant is greater than the etching rate of the contact layer 30 by the acid etching etchant.

[0028] refer to Figure 4 As shown, the electrostatic chuck 1 includes a substrate 10, an electrode layer 20, a contact layer 30 and a film 40. Applicable materials for the substrate include ceramic materials such as aluminum nitride (AlN), aluminum oxide (Al2O3), silicon carbide (SiC), boron nitride (BN), zirconium oxide (ZrO2) and their compounds. The substrate is formed by sintering using existing technology, which is well known to those skilled in the art, and the specific details are not repeated here; the substrate 10 has a relative upper surface 10a and a lower surface 10b, and the electrode layer 20 is arranged on the upper surface 10a of the substrate 10. Applicable electrode layer materials can be high melting point metals or metal alloy materials, such as molybdenum, tungsten and their compounds; the electrode layer 20, the contact layer 30 and the film 40 are stacked on the substrate 10 in sequence; preferably, refer to Figure 4As shown, the electrode layer 20 may be partially covered on the upper surface 10a of the substrate 10, and the contact layer 30 covers the top surface 20a and the side surface 20b of the electrode layer 20 and at the same time covers the upper surface 10a of the substrate 10 not covered by the electrode layer 20; the material applicable to the contact layer may also be aluminum nitride (AlN), aluminum oxide (Al2O3), silicon carbide (SiC), boron nitride (BN), zirconium oxide (ZrO2) and other ceramic materials and their compounds. The contact layer 30 is formed by sintering by existing technology and is well known to those skilled in the art. The specific details are not repeated here; the material applicable to the film may be a material that is easily acid-eroded and resistant to plasma corrosion. oxide material; thus, preferably, the material of the film is selected from Group IIIB metal compounds, or Group IVB metal compounds, or Group IIIA metal compounds, or Group IVA non-metallic compounds, or a combination of the above compounds. For example, the material suitable for the film can be yttrium oxide (Y2O3), aluminum oxide (Al2O3), aluminum nitride (AlN), silicon oxide (SiO2), silicon nitride (Si3N4), titanium nitride (TiN), diamond-like carbon or the above composite materials, so that the film is easier to remove to form a new film; the film can be formed by vacuum coating technology, such as CVD (Chemical Vapor Deposition) / PVD (Physical Vapor Deposition) / ALD (Atomic Layer Deposition) and other processes, which is easy to form quickly and the formed film has high purity, dense structure, and greatly improved or enhanced resistivity and other properties.

[0029] It should be noted that, in this embodiment, a thin film is formed by vapor deposition on the surface of the contact layer formed based on sintering, so that the thin film has more excellent density, and can physically separate the polymers and pollutants generated in the process from the original ceramic layer of the electrostatic suction cup, and the thin film also has more excellent adhesion on the contact layer and will not fall off during use; and the difference in etching rate of the etchant between the thin film and the contact layer makes it easier to remove it using chemical reagents. Not only is the removal method simple, but the polymers and pollutants on the surface can also be removed at the same time during removal. The contact layer is sintered as a whole and is extremely dense. The process of removing the thin film will hardly affect the contact layer, and the surface of the contact layer after the thin film is removed can be coated again to achieve the purpose of repeated cleaning and utilization, thereby greatly extending the service life of the electrostatic suction cup.

[0030] In summary, the present invention proposes to use additive manufacturing to uniformly grow one or more thin films on the contact layer of the electrostatic chuck. After the electrostatic chuck is used, the contaminated film can be removed. Due to the difference in etching rates of the etchant between the formed contact layer and the film, the film can be removed by acid etching without damaging the contact layer. After removal, a new film can be re-plated, thereby extending the service life of the electrostatic chuck.

[0031] In one embodiment, the ratio of the etching rate of the thin film by the acid etching etchant to the etching rate of the contact layer by the acid etching etchant is greater than 100:1. Under this etching rate difference, the contact layer and the thin film are easier to be separated by acid etching, thereby making it easier to clean the thin film on the contact layer.

[0032] In one embodiment, the average grain size of the contact layer is greater than the average grain size of the film; preferably, the contact layer has an average grain size of more than 0.5 μm and less than 5.0 μm; and / or the film has an average grain size of more than 0.04 μm and less than 0.06 μm. The average grain size of the contact layer can be 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0 μm, or any point value between the above two; the film can be 0.04, 0.045, 0.05, 0.055, 0.06 μm, or any point value between the above two; under the difference of these average grain sizes, the film located on the contact layer can be more easily cleaned.

[0033] In one embodiment, the thickness of the film is greater than 0.5 μm and less than 50.0 μm; the thickness of the film 40 can be 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0 μm, or 10.0, 15.0, 20.0, 25.0, 30.0, 35.0, 40.0, 45.0, 50.0 μm, or any point value between two of the above; the thickness of the film should not be too thick, which will easily affect its adhesion to the contact layer and make the electrostatic adsorption force worse, and if it is too thin, it will be difficult to play the role required for setting the film.

[0034] In one embodiment, the contact layer is an insulating layer, and the thin film is made of an insulating oxide material; or the contact layer is a conductive layer, and the thin film is made of a conductive oxide material.

[0035] In one embodiment, the ratio of the resistivity of the film to the resistivity of the contact layer is less than or equal to 5:1; since the electrostatic chuck needs to apply voltage to implement adsorption, if the resistivity of the intermediate film is too high or low, it will affect the adsorption performance. Preferably, the resistivity of the contact layer and the film layer should be at the same order of magnitude. Therefore, the present application has found through experiments that the resistivity of the two is 5:1 or less, which can fully meet the adsorption effect required by the electrostatic chuck; Preferably, the ratio of the resistivity of the film to the resistivity of the contact layer is 1:1.

[0036] In one embodiment, the contact layer is formed by sintering, and the thin film is formed by vacuum evaporation. The present invention prepares the contact layer and the thin film by sintering and vacuum evaporation, respectively, so that the etching rate of the thin film by the acid etching etchant is greater than the etching rate of the contact layer by the acid etching etchant.

[0037] In one embodiment, reference Figure 5 As shown, the film 40 is a multi-layer film structure, and the multi-layer film structure includes a bottom film 41 close to the contact layer and a surface film 42 away from the contact layer; the porosity of the bottom film 41 is greater than that of the surface film 42; When the film is a multi-layer film structure, the porosity of the bottom film is greater than that of the surface film, thereby playing a role in stress release, improving the adhesion of the surface film, and making it less likely to peel off under the expansion stress of high and low temperature differences; the surface film has a small porosity and is therefore denser, better in corrosion resistance, and can play a better protective role. Preferably, the porosity of the bottom film is above 1.0‰ and below 5.0‰, and the porosity of the surface film is below 0.1‰; the porosity of the bottom film 41 can be 1.0‰, 1.5‰, 2.0‰, 2.5‰, 3.0‰, 3.5‰, 4.0‰, 4.5‰, 5.0‰, or any point value between any two of the above; preferably, the material of the bottom film is aluminum oxide, and the material of the surface film is yttrium oxide, wherein yttrium oxide has good plasma corrosion resistance, while aluminum oxide has high hardness, high resistivity, high thermal conductivity and other characteristics. Therefore, the surface film is formed of yttrium oxide material, which has better corrosion resistance and can play a better protective role, while the bottom film is aluminum oxide, which can improve the overall performance of the electrostatic suction cup.

[0038] refer to Figure 1-4 An embodiment of the present invention provides a method for manufacturing the electrostatic chuck, comprising the following steps: Step 1. Reference Figure 1As shown, a substrate 10 is provided; applicable materials of the substrate 10 include ceramic materials such as aluminum nitride (AlN), aluminum oxide (Al2O3), silicon carbide (SiC), boron nitride (BN), zirconium oxide (ZrO2) and their compounds. The substrate can be formed by sintering by existing technology, which is well known to those skilled in the art, and the specific details are not repeated here; Step 2: Reference Figure 2-3 As shown, an electrode layer 20 and a contact layer 30 are sequentially formed and stacked on the substrate 10; the applicable electrode layer material can be a high melting point metal or metal alloy material, such as molybdenum, tungsten and their compounds; the applicable contact layer material can also be aluminum nitride (AlN), aluminum oxide (Al2O3), silicon carbide (SiC), boron nitride (BN), zirconium oxide (ZrO 2) The contact layer 30 is formed by sintering using conventional techniques, which are well known to those skilled in the art, and the specific details are not described here. Step 3. Reference Figure 4 As shown, a thin film 40 is deposited on the contact layer 30; the material of the thin film is selected from a group IIIB metal compound, or a group IVB metal compound, or a group IIIA metal compound, or a group IVA non-metal compound, or a combination of the above compounds. For example, the material suitable for the thin film can be yttrium oxide (Y2O3), aluminum oxide (Al2O3), aluminum nitride (AlN), silicon oxide (SiO2), silicon nitride (Si3N4), titanium nitride (TiN), diamond-like carbon, or a composite material thereof. The thin film can be formed by vacuum coating technology, such as chemical vapor deposition or physical vapor deposition. It is easy to form quickly and the formed thin film has high purity of components, dense structure, and greatly improved or enhanced resistivity and other properties. In particular, it can form an etchant etching rate difference between the contact layer and the thin film, and then the thin film can be removed by acid etching without damaging the contact layer, and a new thin film can be re-plated after removal, thereby extending the service life of the electrostatic chuck. In one embodiment, reference Figure 5 As shown, the film is a multi-layer film structure, and each layer of the film can be formed in sequence, which will not be described in detail here.

[0039] refer to Figure 6 As shown, the present invention provides a method for reusing an electrostatic chuck, the method comprising the following steps: Step 1, forming a patterned mask to protect the chemically corroded portion of the electrostatic chuck and expose the contact layer and the film; specifically, this step mainly masks the sensitive parts of the electrostatic chuck, which include but are not limited to metal, glue, etc.; Step 2, performing acid etching on the contact layer and the thin film to remove the thin film; the acid etching includes immersion, spraying, or horizontal rinsing, wherein the etchant is selected from hydrofluoric acid and / or nitric acid; Due to the difference in etching rates of the formed contact layer and the film, the acid etching rate of the film is greater than the acid etching rate of the contact layer, so that the contact layer is less susceptible to corrosion, thereby extending the service life of the electrostatic chuck.

[0040] Step 3, cleaning and drying the electrostatic chuck after removing the film; Step 4: forming a thin film on the contact layer. The thin film can still be formed by vacuum coating technology, such as chemical vapor deposition or physical vapor deposition, which will not be elaborated here.

[0041] The present invention provides the following test method for the acid etching rate and selectivity ratio of the contact layer and the film; The instruments used include: analytical balance (1 / 10,000), drying oven; The reagents used include: nitric acid (concentration about 10%); The test method includes the following steps: S1. Take the electrostatic chuck samples with and without film as the experimental group and control group respectively, and clean the surface with a dust-free cloth.

[0042] S2. Place the sample in an oven and dry it at 120°C for 1-2 hours. After cooling to room temperature, weigh it with an analytical balance and record it. Repeat the drying and weighing steps until the sample reaches a constant weight, which is the mass m1 before the reaction.

[0043] S3. Place the sample in nitric acid and soak for 20 hours to allow the acid to fully react with the sample surface.

[0044] S4. Take the sample out of the acid, rinse it with pure water three times, wipe it with a dust-free cloth, put it in an oven and dry it at 120°C for 1-2 hours, cool it to room temperature, and weigh it with an analytical balance. Repeat the drying and weighing steps until the constant weight is reached. The constant weight is the mass m2 after the reaction with the acid.

[0045] S5. Calculate the etching rate of the sample and the acid, as well as the selectivity of the surface with or without a film and the acid reaction.

[0046] The etching rate of sample and acid v = (m2-m1) / t; The selectivity ratio of the reaction between the film surface and the acid is k=V 有薄膜 / V 无薄膜 .

[0047] The electrostatic chuck provided by the present invention uniformly grows one or more layers of thin film on the contact layer, and the thin film has good compactness, and can physically separate the polymer and pollutants generated in the process from the original contact layer of the electrostatic chuck; the thin film has good adhesion and will not fall off during the service life; the thin film can be prepared by using ceramic materials such as yttrium oxide, aluminum oxide, aluminum nitride, etc., and has the characteristic of anti-plasma etching; the etching rate of the thin film by the etchant for acid etching is greater than the etching rate of the contact layer by the etchant for acid etching, so that the contact layer of the original electrostatic chuck will not be affected in the process of removing the thin film; after the thin film is removed from the electrostatic chuck provided by the present invention, a thin film can be plated again on the contact layer of the electrostatic chuck, so as to achieve the purpose of repeated cleaning and utilization, and extend the service life of the electrostatic chuck.

[0048] In addition, those skilled in the art should understand that, although there are many problems in the prior art, each embodiment or technical solution of the present invention can be improved in only one or several aspects, without having to solve all the technical problems listed in the prior art or background technology at the same time. Those skilled in the art should understand that the content not mentioned in a claim should not be used as a limitation on the claim.

[0049] Although the terms such as electrostatic chuck, substrate, upper surface, lower surface, electrode layer, top surface, side, contact layer, film, bottom film, surface film, etc. are used more frequently in this article, the possibility of using other terms is not excluded. These terms are used only to more conveniently describe and explain the essence of the present invention; interpreting them as any additional restrictions is contrary to the spirit of the present invention; the terms "first", "second", etc. (if any) in the description and claims of the embodiments of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence.

[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An electrostatic chuck, It is characterized in that The electrostatic chuck includes: substrate; and An electrode layer, a contact layer and a thin film are sequentially stacked on the substrate; The etching rate of the thin film by the acid etching etchant is greater than the etching rate of the contact layer by the acid etching etchant.

2. The electrostatic chuck according to claim 1, Features: The ratio of the etching rate of the thin film by the acid etching etchant to the etching rate of the contact layer by the acid etching etchant is greater than 100:

1.

3. The electrostatic chuck according to claim 1, Features: The material of the film is an oxide material that is easily corroded by acid and resistant to plasma corrosion.

4. The electrostatic chuck according to claim 1, Features: The thickness of the thin film is greater than or equal to 0.5 μm and less than or equal to 50.0 μm.

5. The electrostatic chuck according to claim 1, Features: The contact layer is formed by sintering, and the thin film is formed by vacuum deposition.

6. A method for reusing the electrostatic chuck according to any one of claims 1 to 5, It is characterized in that The method comprises the following steps: forming a patterned mask to protect the portion of the electrostatic chuck susceptible to chemical corrosion and to expose the contact layer and the thin film; performing acid etching on the contact layer and the thin film to remove the thin film; cleaning and baking the electrostatic chuck after removing the film; A thin film is formed on the contact layer.

7. The method of use according to claim 6, Features: The acid etching includes immersion type, spray type, or horizontal rinsing type, wherein the etchant used for the acid etching is selected from hydrofluoric acid and / or nitric acid.

8. The method of use according to claim 7, Features: The acid etching rate of the thin film is greater than the acid etching rate of the contact layer.