Field effect transistor of one-dimensional black phosphorus nanobelt or phosphorene nanobelt prepared based on liquid phase stripping and cascade centrifugation method
Through the combined design of liquid phase peeling and step centrifugation method and graphene and boron nitride electrodes, the problems of high cost, low yield and easy oxidation of one-dimensional black phosphorus nanobelt field effect transistors in the prior art are solved, and high efficiency is achieved , uniform nanoribbon preparation and performance improvement.
Patent Information
- Application Number
- CN202411198419.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, the preparation of one-dimensional black phosphorus nanoribbon or phosphorene nanoribbon field effect transistors has problems such as high cost, low yield, many edge defects, many heteroatoms, and low-dimensional black phosphorus is prone to oxidation and degradation.
The liquid phase peeling and step-connected centrifugal method are used to prepare one-dimensional black phosphorus nanoribbons or phosphorene nanoribbons. Combined with the design of graphene contact electrode and boron nitride top gate electrode, the surface is separated by ultrasonic peeling and different centrifugal velocities to form a clean surface. Neatly edged nanoribbons and reduced oxidation by boron nitride protection.
A field-effect transistor with low cost, high yield, nanoribbon size uniformity and excellent performance is achieved, reducing Schottky barrier and oxidation risks, and improving device performance.
Smart Images

Figure CN119069532A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of field effect transistors (FET), and in particular to a field effect transistor of a one-dimensional black phosphorus nanoribbon or phosphorene nanoribbon prepared by a liquid phase exfoliation and cascade centrifugation method. Background Art
[0002] In 2014, Chen Xianhui's research group cooperated with Zhang Yuanbo's research group to use tape for mechanical exfoliation to peel black phosphorus (BP) flakes from bulk single crystals, and fabricated field effect transistors based on them. When the thickness of the two-dimensional black phosphorus material is 10nm, the field effect transistor has a performance of 10 5 The on / off ratio is about 600 cm at 25°C. 2 ·V -1 ·s -1 , reaching 1000cm at 120K or lower 2 ·V -1 ·s -1 , showing the great potential of two-dimensional black phosphorus field-effect transistors in the application of nanoelectronic devices. This study has attracted widespread attention from researchers to two-dimensional black phosphorus in the field of optical and electrical devices.
[0003] Compared with two-dimensional black phosphorus (2D BP), one-dimensional black phosphorus nanoribbons (BPNR) or one-dimensional phosphorene nanoribbons (PNR) have smaller size, more significant edge effect, higher specific surface area, stronger quantum confinement effect and direction dependence, which can lead to new physical phenomena and applications. For example, more significant anisotropic thermal conductivity, mechanical properties and electrical properties, as well as novel room temperature edge magnetism and planar ferroelectric polarization, etc., which makes one-dimensional black phosphorus nanoribbons and one-dimensional phosphorene nanoribbons have application prospects in the field of optoelectronic devices.
[0004] In optoelectronic devices, the quality of the black phosphorus nanoribbons or phosphorene nanoribbons used, such as thickness, neat edges, and clean surfaces, is very important. However, the preparation of black phosphorus nanoribbons or phosphorene nanoribbons with clean surfaces, neat edges, and thin layers is still a major challenge. At present, the preparation methods of black phosphorus nanoribbons can be mainly divided into three categories: the first category is to use high-energy electron beams to cut large areas of black phosphorus into nanoribbons. Although this type of preparation method can obtain BPNR or PNR, it requires expensive equipment, low yield, and is severely limited by processing accuracy. The edge structure of the prepared BPNR or PNR is messy. At the same time, due to exposure to high-energy particles, there are some defects in the nanoribbon structure, which will affect the intrinsic properties of the nanoribbon. The second category is to directly grow black BPNR or PNR by chemical vapor transport (CVD). This method has the disadvantages of having a large number of layers of black phosphorus nanoribbons and difficult to control thickness due to the difficulty in accurately controlling the growth conditions. The third category is to use liquid phase exfoliation to strip BPNR or PNR from thick layers of black phosphorus raw materials. However, the existing liquid phase exfoliation method has the disadvantages of low yield of single-layer phosphorene in phosphorene, uncontrollable size and morphology of the prepared phosphorene, difficulty in preparing phosphorene with one-dimensional strip morphology, and uneven width of the prepared BPNR or PNR.
[0005] In addition, low-dimensional black phosphorus still faces two challenges in the application of field effect transistor devices. First, when the semiconductor contacts the metal electrode, a Schottky barrier and Fermi pinning effect will be formed, making it difficult for FET devices to achieve good ohmic contact; second, low-dimensional black phosphorus is easily oxidized and degraded in the air. This is because after the phosphorus atom in its molecular structure forms a bond with the other three phosphorus atoms, the phosphorus still has a pair of free lone pairs of electrons. The lone pair of electrons is active and can be easily taken away by oxygen molecules, causing the oxidation of the outer layer of black phosphorus. In the presence of water, the phosphorus oxide generated on the surface will quickly react with water to generate phosphoric acid and degrade. The exposed black phosphorus will continue to be oxidized and degraded.
[0006] In summary, field effect transistor devices based on low-dimensional black phosphorus and their preparation methods are still the focus of research for technicians in this field. Summary of the invention
[0007] The object of the present invention is to provide a field effect transistor based on a one-dimensional black phosphorus nanoribbon (BPNR) or phosphorene nanoribbon (PNR) prepared by a liquid phase exfoliation and cascade centrifugation method, so as to solve the above problems existing in the prior art.
[0008] To achieve the above object, the present invention provides the following solutions:
[0009] One of the technical solutions of the present invention: a field effect transistor based on one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon, characterized in that it includes a target substrate, a graphene contact electrode, a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon channel, a source and a drain electrode, and a boron nitride (BN) top gate electrode arranged in sequence; the one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon is prepared by liquid phase exfoliation and cascade centrifugation method.
[0010] Furthermore, the graphene contact electrodes are located on the surface of the target substrate and are two adjacent graphene contact electrodes arranged correspondingly, and the straight-line distance between the two adjacent graphene contact electrodes is 10 nm to 100 μm.
[0011] Furthermore, the graphene contact electrode is located between the target substrate and the one-dimensional BPNR or one-dimensional PNR channel, that is, the one-dimensional BPNR or one-dimensional PNR channel is located above the target substrate, and the two ends are overlapped on the surfaces of two adjacent graphene contact electrodes; the source and drain electrodes are respectively located on the two side edges of the surfaces of two adjacent graphene contact electrodes (the side schematic diagram is shown in FIG. Figure 6 shown).
[0012] Furthermore, the thickness of the graphene contact electrode is 0.3-10 nm; and the boron nitride top gate electrode is a single-layer boron nitride.
[0013] Furthermore, the one-dimensional BPNR or one-dimensional PNR channel has a thickness of 0.5 to 20 nm, a width of 1 to 300 nm, and a length of 500 nm to 900 μm.
[0014] Technical solution 2 of the present invention: The method for preparing the above field effect transistor comprises the following steps:
[0015] (A) preparing a positioning mark on a substrate to obtain a target substrate with the positioning mark;
[0016] (B) transferring graphene to the surface of the target substrate with the positioning mark, and patterning the graphene to obtain a graphene contact electrode; the straight-line distance between two adjacent patterned graphene contact electrodes is 10 nm to 100 μm;
[0017] (C) Using black phosphorus crystals as raw materials, one-dimensional BPNR or one-dimensional PNR was prepared by liquid phase exfoliation and cascade centrifugation method;
[0018] (D) transferring the one-dimensional BPNR or one-dimensional PNR as a channel of a field effect transistor to the surface of the graphene contact electrode;
[0019] (E) accurately locating the position where the one-dimensional BPNR or one-dimensional PNR contacts the graphene contact electrode through the positioning mark on the target substrate, and then making the source and drain electrodes on the surface of the graphene contact electrode respectively;
[0020] (F) A layer of boron nitride is transferred as a top gate electrode on the surface of the one-dimensional BPNR or one-dimensional PNR and on the surface of the graphene contact electrode that is not covered by the source and drain electrodes.
[0021] Furthermore, the step (A) specifically includes: spin coating a 0.1-50 μm thick photoresist on the substrate surface, and drying at 100-150° C. for 1-10 min; using a patterned mask with a positioning function to ultraviolet-expose the substrate surface for 5s-10min, developing, and drying; using a thermal evaporation or electron beam evaporation process to evaporate a 20-300nm thick metal on the substrate surface after ultraviolet exposure and development to obtain a target substrate with a positioning mark.
[0022] Furthermore, the step (A) further comprises:
[0023] The substrate is a rigid substrate or a flexible substrate; the rigid substrate includes a silicon substrate with a silicon dioxide layer on the surface, a sapphire substrate, a ceramic substrate, a mica substrate, an ITO conductive glass substrate, a quartz glass substrate or a soda-lime glass substrate; the flexible substrate includes a polyamide (PI) resin film or a polyethylene terephthalate (PET) resin film.
[0024] The photoresist includes but is not limited to PrMat 5214.
[0025] The specific operation of the development is: soaking or rinsing in a developer or deionized water for 1 to 10 minutes respectively.
[0026] The metals evaporated on the surface of the substrate after ultraviolet exposure and development by thermal evaporation or electron beam evaporation process include but are not limited to gold, silver, copper, nickel, platinum, aluminum, chromium, titanium, molybdenum, zinc, magnesium, bismuth, zirconium, cadmium, barium, iron, cobalt, niobium, tungsten, indium, indium tin oxide, etc. and a combination of any two or three of them, such as a titanium / gold composite layer, a chromium / gold composite layer or a titanium / gold / titanium composite layer.
[0027] After the metal is evaporated, the substrate with the metal on the surface is immersed in acetone for 0.5 to 24 hours, ultrasonically vibrated for 5 seconds to 60 minutes, and then rinsed with isopropyl alcohol and blown dry.
[0028] The drying is carried out by blowing with nitrogen or argon.
[0029] Furthermore, the step (B) specifically includes: soaking the graphene in a 0.1-1 mol / L ammonium persulfate solution for 1-24 hours, rinsing with clean water and then transferring it to the surface of the target substrate with the positioning mark described in step (A), and drying it at 20-60° C. for 2-24 hours to obtain a graphene layer; spin coating a 0.1-50 μm thick photoresist on the surface of the graphene layer, and drying it at 100-150° C. for 1-10 minutes; using a patterned mask to ultraviolet expose the surface of the graphene layer for 5 seconds to 10 minutes, developing, and drying; using oxygen plasma or argon ion beam to etch the ultraviolet exposed and developed graphene layer to pattern it to obtain a graphene contact electrode.
[0030] Furthermore, the step (B) further comprises:
[0031] The drying at 20-60° C. for 2-24 hours further includes soaking in acetone for 2-10 hours, washing with isopropanol 1-3 times, and then drying again at 20-60° C. for 2-24 hours.
[0032] The photoresist includes but is not limited to PrMat 5214.
[0033] The specific operation of the development is: soaking or rinsing in a developer or deionized water for 1 to 10 minutes respectively.
[0034] The etching parameters include: etching power of 20-200W, etching time of 10s-30min, and gas flow rate of 0.1-300sccm.
[0035] The drying is carried out by blowing with nitrogen or argon.
[0036] The straight-line distance between two adjacent patterned graphene contact electrodes is 10 nm to 100 μm.
[0037] Furthermore, the step (C) specifically includes: mixing black phosphorus crystals and an organic solvent to obtain a mixed solution; ultrasonically treating the mixed solution for 1 to 12 hours to obtain a black phosphorus dispersion; centrifuging the black phosphorus dispersion at centrifugal speeds of 2000r / min, 4000r / min, 6000r / min, 8000r / min, 12000r / min, and 14000r / min for 1 hour each, and using a pipette to aspirate the upper clear liquid after centrifugation in the centrifuge tube to obtain a one-dimensional BPNR or a one-dimensional PNR.
[0038] Furthermore, the step (C) further comprises:
[0039] The usage ratio of the black phosphorus crystals to the organic solvent is 0.001-100 g: 5-100 mL.
[0040] The organic solvent includes methanol, ethanol, acetone, isopropanol, dimethyl sulfoxide or N,N-dimethylformamide.
[0041] During the ultrasonic treatment, a circulating water condensation system was used to cool the water temperature and control the ultrasonic temperature below 30°C.
[0042] The ultrasonic treatment is carried out under the protection of an inert gas such as nitrogen or argon.
[0043] The one-dimensional BPNR or one-dimensional PNR has a thickness of 0.5 to 20 nm and a width of 1 to 300 nm.
[0044] The one-dimensional BPNR or one-dimensional PNR has a length of 500 nm to 900 μm.
[0045] The one-dimensional BPNR or one-dimensional PNR prepared by the above method has neat edges and clean surfaces.
[0046] When the supernatant after centrifugation in the centrifuge tube is sucked with a pipette, the width and thickness ranges of the one-dimensional BPNR or one-dimensional PNR obtained when the supernatant is sucked at different heights from the surface are different (the supernatant obtained when sucking at different heights from the surface may be one-dimensional BPNR or one-dimensional PNR, or a mixture of one-dimensional BPNR and one-dimensional PNR), which can be observed and counted using a scanning electron microscope; when the supernatant is sucked 0.5 cm away from the surface with a pipette, the length of the one-dimensional BPNR or one-dimensional PNR obtained is 1 to 2 μm, the width is 30 to 50 nm, and the thickness is 0.5 to 10 nm; when the supernatant is sucked 2 cm away from the surface with a pipette, the length of the one-dimensional BPNR or one-dimensional PNR obtained is 5 to 30 μm, the width is 50 to 100 nm, and the thickness is 0.5 to 15 nm.
[0047] Further, the step (D) specifically comprises: transferring the one-dimensional BPNR or one-dimensional PNR to the surface of the graphene contact electrode, -3 ~10 -5 Pa vacuum and heat at 30-80°C for 2-24h.
[0048] Furthermore, the step (D) further comprises:
[0049] The transfer is specifically to transfer the dispersion of one-dimensional BPNR or one-dimensional PNR (or directly absorb the upper clear liquid after centrifugation in the centrifuge tube) to the surface of the graphene contact electrode by spin coating, dripping, inkjet printing, screen printing or dry method using a microscope transfer platform. Finally, it is ensured that at least one one-dimensional BPNR or one one-dimensional PNR is successfully transferred to the surfaces of two adjacent graphene contact electrodes (the two ends are overlapped on the surfaces of two adjacent graphene contact electrodes).
[0050] After the heating is completed, the step of cleaning with acetone and isopropanol is also included.
[0051] Furthermore, the step (E) specifically includes: using a scanning electron microscope to observe the position where the one-dimensional BPNR or one-dimensional PNR contacts the graphene contact electrode; spin coating an electron photoresist with a thickness of 0.5 to 10 μm on the surface of the one-dimensional BPNR or one-dimensional PNR and the surface of the graphene contact electrode, and drying at 100 to 150° C. for 1 to 10 minutes; patterning the source and drain electrodes on the surface of the graphene contact electrode through an electron beam lithography process, and developing and drying; and evaporating a 30 to 100 nm thick metal on the surface of the graphene contact electrode after the source and drain electrodes are patterned to form source and drain electrodes.
[0052] Furthermore, the step (E) further comprises:
[0053] The electronic photoresist includes but is not limited to PMMA950K.
[0054] The specific operation of the development is: soaking or rinsing in a developer or deionized water for 1 to 10 minutes respectively.
[0055] After the metal is evaporated, the process also includes soaking in acetone for 0.5 to 24 hours, ultrasonically oscillating for 5 seconds to 30 minutes, rinsing with isopropyl alcohol, and drying.
[0056] The metals include, but are not limited to, gold, silver, copper, nickel, platinum, aluminum, chromium, titanium, molybdenum, zinc, magnesium, bismuth, zirconium, cadmium, barium, iron, cobalt, niobium, tungsten, indium, indium tin oxide, etc., and composite layers of any two or three thereof, such as titanium / gold composite layers, chromium / gold composite layers, or titanium / gold / titanium composite layers, etc.
[0057] The drying is carried out by blowing with nitrogen or argon.
[0058] Further, the step (F) specifically includes: mechanically exfoliating the boron nitride block to obtain a mixture of single-layer, double-layer, triple-layer, and few-layer boron nitride, transferring it to the surface of the PDMS substrate, and then using a microscope transfer platform to press the single-layer boron nitride on the surface of the PDMS substrate onto the one-dimensional BPNR or one-dimensional PNR channel and the part of the graphene contact electrode that is not covered by the source and drain electrodes to form a top gate electrode; and then placing it at 10 -3 ~10 -5 The field effect transistor is obtained by annealing at 100-200° C. for 30-300 min under a vacuum of 0.04 Pa.
[0059] The present invention aims at the disadvantages of high cost, low yield, many edge defects and many heteroatoms of BPNR or PNR field effect transistors prepared by the prior art, and proposes a one-dimensional BPNR or PNR field effect transistor prepared by liquid phase exfoliation and cascade centrifugation method and a preparation method thereof, including a method for preparing one-dimensional BPNR or PNR by liquid phase exfoliation and cascade centrifugation method, and a preparation method of a field effect transistor based on one-dimensional BPNR or PNR, wherein the field effect transistor structure is divided into a target substrate, a one-dimensional BPNR or one-dimensional PNR channel, a graphene contact electrode, a metal source and drain electrode, and a boron nitride top gate electrode. The method for preparing one-dimensional BPNR or one-dimensional PNR by liquid phase exfoliation and cascade centrifugation method in the present invention has the advantages of low cost, high yield, pure product and uniform size. The design of using graphene as the contact electrode and boron nitride as the top gate electrode in the field effect transistor of the present invention is conducive to reducing the contact resistance between the semiconductor BPNR or PNR and the metal electrode, reducing the Schottky barrier, and the design of boron nitride as the top gate is conducive to physical protection of BPNR and PNR that are prone to oxidation.
[0060] The present invention discloses the following technical effects:
[0061] The present invention provides a field effect transistor based on a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon, comprising a target substrate, a graphene contact electrode, a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon channel, a source electrode, a drain electrode and a boron nitride top gate electrode arranged in sequence; the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon is prepared by a liquid phase exfoliation and cascade centrifugation method. The field effect transistor of the present invention uses a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon prepared by a special liquid phase exfoliation and cascade centrifugation method as a channel, and the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon prepared by a special liquid phase exfoliation and cascade centrifugation method has the advantages of a clean surface, neat edges, a single crystal structure, and relatively uniform size, which is conducive to improving device performance. The principle of the present invention to obtain one-dimensional BPNR or one-dimensional PNR with such characteristics by using liquid phase exfoliation and cascade centrifugation method is that: first, no surfactant or salt is added in the ultrasonic exfoliation process to reduce the introduction of impurities, and the ultrasonic wave generates high-temperature and high-pressure bubbles in the solution. When these bubbles collapse, microjets and shock waves are generated. The microjets and shock waves generated under appropriate power and time are more likely to make the BP crystal tend to be exfoliated along the (001) crystal plane, rather than along other crystal planes, thereby forming a one-dimensional BPNR or PNR. These BPNR or PNR have a zigzag edge orientation, which is naturally formed by exfoliation along the (001) crystal plane; second, the cascade centrifugation method used uses different centrifugal speeds and times to separate BPNR or PNR of different sizes step by step, so that the surface of the obtained product is clean and uniform in size. In addition, the design of the graphene contact electrode of the present invention is conducive to reducing the contact resistance between the semiconductor one-dimensional BPNR or one-dimensional PNR and the metal electrode, reducing the Schottky barrier, and the design of boron nitride as the top gate is conducive to physical protection of BPNR and PNR that are prone to oxidation. The above factors work together to make the field effect transistor of the present invention have excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0063] Figure 1 is a SEM photograph of the Si / SiO2 target substrate with positioning marks in Example 1;
[0064] Figure 2 This is an SEM photo of the graphene contact electrode (graphene after patterning) and its region enlarged in Example 1;
[0065] Figure 3This is a SEM photograph of the one-dimensional BPNR in the supernatant at 0.5 cm from the liquid surface after liquid phase exfoliation and cascade centrifugation in Example 1;
[0066] Figure 4 This is a SEM photograph of the one-dimensional BPNR in the supernatant 2 cm away from the liquid surface after liquid phase exfoliation and cascade centrifugation in Example 1;
[0067] Figure 5 This is a selected area electron diffraction (SAED) photograph of one-dimensional BPNR in the supernatant 2 cm away from the liquid surface after liquid phase exfoliation and cascade centrifugation in Example 1;
[0068] Figure 6 It is a side schematic diagram of a field effect transistor prepared in Example 1 with one-dimensional BPNR as a channel, graphene as a contact electrode, and boron nitride as a top gate;
[0069] Figure 7 It is a side schematic diagram of a field effect transistor prepared in Comparative Example 1 with a one-dimensional BPNR as a channel and graphene as a contact electrode;
[0070] Figure 8 It is a side schematic diagram of a field effect transistor prepared in Comparative Example 2 with one-dimensional BPNR as a channel, graphene as a contact electrode, and Al2O3 as a top gate;
[0071] Fig. 9 This is a side schematic diagram of a field effect transistor prepared in Comparative Example 3 with a one-dimensional BPNR as a channel and boron nitride as a top gate. DETAILED DESCRIPTION
[0072] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0073] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0074] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0075] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0076] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0077] The present invention provides a field effect transistor based on a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon, comprising a target substrate, a graphene contact electrode, a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon channel, a source electrode, a drain electrode and a boron nitride top gate electrode which are arranged in sequence; the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon is prepared by a liquid phase exfoliation and cascade centrifugation method.
[0078] The present invention also provides a method for preparing the above field effect transistor, comprising the following steps:
[0079] (A) preparing a positioning mark on a substrate to obtain a target substrate with the positioning mark;
[0080] (B) transferring graphene to the surface of the target substrate with the positioning mark, and patterning the graphene to obtain a graphene contact electrode; the straight-line distance between two adjacent patterned graphene contact electrodes is 10 nm to 100 μm;
[0081] (C) Using black phosphorus crystals as raw materials, one-dimensional black phosphorus nanoribbons or one-dimensional phosphorene nanoribbons are prepared by liquid phase exfoliation and cascade centrifugation method;
[0082] (D) transferring the one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon as a channel of a field effect transistor to the surface of the graphene contact electrode;
[0083] (E) accurately locating the position where the one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon contacts the graphene contact electrode through the positioning mark on the target substrate, and then making source and drain electrodes on the surface of the graphene contact electrode respectively;
[0084] (F) A layer of boron nitride is transferred onto the surface of the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon and the surface of the graphene contact electrode that is not covered by the source and drain electrodes as a top gate electrode.
[0085] As a preferred embodiment of the present invention, the preparation method more specifically comprises the following steps:
[0086] (A) preparing a positioning mark on a substrate to obtain a target substrate with the positioning mark, specifically comprising:
[0087] S1. Spin-coat a 0.1 μm to 50 μm thick photoresist (including but not limited to PrMat 5214) on the substrate surface and dry it on a hot plate at 100 to 150° C. for 1 to 10 min;
[0088] S2. Exposure and development: using a patterned mask with a positioning function and a UV exposure device to expose the substrate surface to UV light for 5s to 10min, and soaking or rinsing in a developer or deionized water for 1 to 10min, and drying with nitrogen or argon;
[0089] S3. Using thermal evaporation or electron beam evaporation process, a 20-300 nm thick metal (including but not limited to gold, silver, copper, nickel, platinum, aluminum, chromium, titanium, molybdenum, zinc, magnesium, bismuth, zirconium, cadmium, barium, iron, cobalt, niobium, tungsten, indium, indium tin oxide, etc. and a composite layer of any two or three thereof, such as a titanium / gold composite layer, a chromium / gold composite layer or a titanium / gold / titanium composite layer, etc.) is evaporated on the surface of the substrate after ultraviolet exposure and development, and the target substrate with metal on the surface is immersed in acetone for 0.5-24 hours, ultrasonically oscillated in an ultrasonic cleaning machine for 5s-60min, the metal other than the positioning mark is removed, and the substrate is taken out, rinsed with isopropanol, and blown dry with nitrogen or argon to obtain a target substrate with positioning marks;
[0090] (B) transferring graphene to the surface of the target substrate with the positioning mark, and patterning the graphene to obtain a graphene contact electrode, specifically comprising:
[0091] S4. Transfer: soak the purchased graphene with polymethyl methacrylate (PMMA) on the surface and copper substrate on the back in a 0.1-1 mol / L ammonium persulfate solution for 1-24 hours to etch away the copper substrate on the back of the graphene, and rinse it in clean water for 3 times to remove the contamination of the graphene by impurity ions; then transfer it to the target substrate surface with positioning marks described in step (A), dry it at 20-60°C for 2-24 hours, and then soak it in acetone at room temperature for 2-10 hours to remove PMMA on the graphene surface, rinse it with isopropanol 1-3 times, and then dry it at 20-60°C for 2-24 hours to obtain a graphene layer;
[0092] S5. Glue coating: Spin-coat a 0.1-50 μm thick photoresist (including but not limited to PrMat5214) on the surface of the graphene layer, and dry it on a hot plate at 100-150° C. for 1-10 min;
[0093] S6. Exposure and development: using a patterned mask with a positioning function and a UV exposure device to expose the graphene layer to UV light for 5 seconds to 10 minutes, and soaking or rinsing in a developer or deionized water for 1 to 10 minutes, respectively, and drying with nitrogen or argon gas;
[0094] S7. Dry etching graphene to pattern it: using oxygen plasma or argon ion beam to etch the graphene layer after ultraviolet exposure and development to pattern it, and obtain graphene contact electrodes; the etching parameters include: etching power of 20 to 200 W, etching time of 10 s to 30 min, gas flow rate of 0.1 to 300 sccm; the straight-line distance between two adjacent patterned graphene contact electrodes is 10 nm to 100 μm;
[0095] (C) Using black phosphorus crystal as raw material, a one-dimensional BPNR or a one-dimensional PNR is prepared by liquid phase exfoliation and cascade centrifugation method, specifically comprising:
[0096] S8. Liquid phase stripping: weigh 0.001-100 g of black phosphorus crystals and put them into a conical flask containing 5-100 mL of an organic solvent (methanol, ethanol, acetone, isopropanol, dimethyl sulfoxide or N,N-dimethylformamide) to obtain a mixed solution; ultrasonically treat the mixed solution in an ultrasonic machine for 1-12 h (ultrasonic power is 30-60 W). During the ultrasonic treatment, a circulating water condensation system is used to cool the water temperature, and the ultrasonic temperature is controlled to be lower than 30°C. Inert gas (such as nitrogen or argon) is used for protection. After the ultrasonic treatment, a BP dispersion is obtained;
[0097] S9. Cascade centrifugation: The BP dispersion was transferred to a centrifuge tube and centrifuged at 2000 r / min, 4000 r / min, 6000 r / min, 8000 r / min, 12000 r / min, and 14000 r / min for 1 h each to remove the precipitate step by step;
[0098] S10. Use a pipette to suck the supernatant of the one-dimensional BPNR or one-dimensional PNR after centrifugation in the centrifuge tube to obtain a one-dimensional BPNR or one-dimensional PNR (thickness of 0.5-20nm, width of 1-300nm, length of 500nm-900μm); when using a pipette to suck the supernatant after centrifugation in the centrifuge tube, the width and thickness ranges of the one-dimensional BPNR or one-dimensional PNR obtained when sucking the supernatant at different heights from the surface are different, and a scanning electron microscope can be used for observation and statistics; when using a pipette to suck the supernatant 0.5cm away from the surface, the length of the one-dimensional BPNR or one-dimensional PNR obtained is 1-2μm, the width is 30-50nm, and the thickness is 0.5-10nm; when using a pipette to suck the supernatant 2cm away from the surface, the length of the one-dimensional BPNR or one-dimensional PNR obtained is 5-30μm, the width is 50-100nm, and the thickness is 0.5-15nm;
[0099] (D) transferring the one-dimensional BPNR or one-dimensional PNR as a channel of a field effect transistor to the surface of the graphene contact electrode, specifically comprising:
[0100] S11. The dispersion of one-dimensional BPNR or one-dimensional PNR (or the supernatant after centrifugation in a centrifuge tube) is directly transferred to the surface of the graphene contact electrode by spin coating, dropwise addition, inkjet printing, screen printing or dry method using a microscope transfer platform;
[0101] S12. Then quickly put it into a vacuum tube furnace and -3 ~10 -5 The dried sample is heated under the conditions of vacuum of 0.04 Pa and 30 to 80° C. for 2 to 24 hours; the dried sample is cleaned with acetone and isopropanol to remove the organic solvent remaining on the surface of the sample;
[0102] (E) accurately locating the position where the one-dimensional BPNR or one-dimensional PNR contacts the graphene contact electrode through the positioning mark on the target substrate, and then making source and drain electrodes on the surface of the graphene contact electrode, respectively, specifically including:
[0103] S13. Observing the contact position of the one-dimensional BPNR or one-dimensional PNR with the graphene contact electrode using a scanning electron microscope (SEM);
[0104] S14. Spin-coat an electronic photoresist (including but not limited to PMMA 950K) with a thickness of 0.5 to 10 μm on the surface of the one-dimensional BPNR or one-dimensional PNR and the surface of the graphene contact electrode, and dry on a hot plate at 100 to 150° C. for 1 to 10 min;
[0105] S15. Patterning source and drain electrodes on the surface of the graphene contact electrode by electron beam lithography (EBL) process, and soaking or rinsing in developer or deionized water for 1 to 10 minutes respectively for development, and drying with nitrogen or argon gas;
[0106] S16. Using thermal evaporation or electron beam evaporation process, 30-100 nm thick metal (including but not limited to gold, silver, copper, nickel, platinum, aluminum, chromium, titanium, molybdenum, zinc, magnesium, bismuth, zirconium, cadmium, barium, iron, cobalt, niobium, tungsten, indium, indium tin oxide, etc. and any two or three of them The composite layer of combination, such as titanium / gold composite layer, chromium / gold composite layer or titanium / gold / titanium composite layer, etc.) is evaporated on the surface of the graphene contact electrode after the source and drain electrodes are patterned to form source and drain electrodes, and then immersed in acetone for 0.5-24 hours, ultrasonically oscillated in an ultrasonic cleaning machine for 5s-30min, taken out, rinsed with isopropanol, and blown dry with nitrogen or argon;
[0107] (F) transferring a layer of boron nitride as a top gate electrode on the surface of the one-dimensional BPNR or one-dimensional PNR and on the surface of the graphene contact electrode that is not covered by the source and drain electrodes, specifically comprising:
[0108] S17. Use blue tape to mechanically peel off the BN block to obtain a mixture of single-layer, double-layer, triple-layer, and few-layer boron nitride, and transfer it to the surface of the PDMS substrate. Then, use a microscope transfer platform to press the single-layer BN on the PDMS substrate onto the surface of the one-dimensional BPNR or one-dimensional PNR channel and the graphene contact electrode that is not covered by the source and drain electrodes to form a top gate electrode;
[0109] S18. Place the above devices at 10 -3 ~10 -5 Annealing is performed at 100-200° C. for 30-300 min under a vacuum of 1.5 Pa to improve the contact between the BPNR or PNR and the graphene contact electrode to obtain a final field effect transistor device.
[0110] The field effect transistor based on one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon and the preparation method thereof of the present invention are further described below in conjunction with specific embodiments.
[0111] Example 1
[0112] A one-dimensional BPNR or one-dimensional PNR top-gate field effect transistor prepared based on liquid phase exfoliation and cascade centrifugation method, the preparation steps are as follows:
[0113] (A) preparing a positioning mark on a substrate to obtain a target substrate with the positioning mark, specifically comprising:
[0114] S1. Prepare a silicon substrate (Si / SiO2) with a size of 1 cm × 1 cm and a 300 nm thick SiO2 oxide layer on the surface; spin-coat a photoresist PrMat 5214 with a thickness of 1 μm on the substrate surface and dry it on a hot plate at 120°C for 90 seconds;
[0115] S2. Exposure and development: The substrate surface is exposed to UV light for 2 min using a patterned mask with positioning function and UV exposure equipment, and then immersed in developer and deionized water for 90 s and 60 s respectively, and then dried with nitrogen;
[0116] S3. A 50nm thick metal layer (5nmTi+45nmAu, Ti is deposited first) is deposited on the surface of the substrate after UV exposure and development by vacuum thermal evaporation. The target substrate with metal on the surface after evaporation is immersed in acetone for 1h, ultrasonically oscillated in an ultrasonic cleaner for 1min, and the metal other than the positioning mark is removed. The substrate is taken out, rinsed with isopropanol, and dried with nitrogen to obtain a target substrate with positioning marks. Its SEM photo is shown as follows: Figure 1 As shown;
[0117] (B) transferring graphene to a target substrate surface with positioning marks, and patterning the graphene to obtain a graphene contact electrode, specifically comprising:
[0118] S4. Transfer: The purchased graphene with PMMA on the surface and copper substrate on the back is soaked in a 1 mol / L ammonium persulfate solution for 4 hours to etch away the copper substrate on the back of the graphene, and rinsed in clean water for 3 times to remove the contamination of the graphene by impurity ions; then transferred to the target substrate surface with positioning marks obtained in step (A), dried at 30°C for 6 hours, and then soaked in acetone at room temperature for 4 hours to remove the protective layer PMMA on the graphene surface, rinsed with isopropanol 3 times and dried again at 30°C for 24 hours to obtain a graphene layer (specifically a single-layer graphene) with a thickness of about 0.3 nm;
[0119] S5. Glue coating: Spin-coat 1 μm thick photoresist PrMat 5214 on the surface of the graphene layer and dry on a hot plate at 120°C for 90 seconds;
[0120] S6. Exposure and development: Use a patterned mask and UV exposure equipment to expose the graphene layer to UV light for 2 min, and soak it in developer and deionized water for 90 s and 60 s respectively, and blow dry with nitrogen;
[0121] S7. Dry etching graphene to pattern it: using an argon ion beam to etch the graphene layer after UV exposure and development to pattern it, and obtain a graphene contact electrode; the etching power is 100 W, the etching time is 5 min, the gas flow rate is 100 sccm, the straight-line distance between two adjacent patterned graphene contact electrodes is 700 nm, and the SEM photo of the prepared graphene contact electrode (i.e., patterned graphene) is as follows Figure 2 As shown;
[0122] (C) Using black phosphorus crystal as raw material, a one-dimensional BPNR or a one-dimensional PNR is prepared by liquid phase exfoliation and cascade centrifugation method, specifically comprising:
[0123] S8. Liquid phase exfoliation: Weigh 10 g of black phosphorus crystals and put them into a conical flask containing 10 mL of organic solvent (dimethyl sulfoxide) to obtain a mixed solution; ultrasonically treat the mixed solution in an ultrasonic cleaning machine for 10 h (ultrasonic power is 30 W). During the ultrasonic treatment, a circulating water condensation system is used to cool the water temperature to control the ultrasonic temperature below 30°C, and an inert gas (nitrogen) is used for protection. After the ultrasonic treatment, a BP dispersion is obtained;
[0124] S9. Stepwise centrifugation: The BP dispersion obtained in step S8 was transferred to a 5 mL centrifuge tube with a dropper, and centrifuged at 2000 r / min, 4000 r / min, 6000 r / min, 8000 r / min, 12000 r / min, and 14000 r / min for 1 h each, and the precipitate was removed step by step;
[0125] S10. Use a pipette to suck the supernatant in the centrifuge tube 0.5 cm away from the surface, and dry it to obtain a mixture of one-dimensional BPNR and one-dimensional PNR. The SEM photo of the mixture is shown in Figure 3 As shown, it can be seen that the one-dimensional BPNR and one-dimensional PNR in the mixture of the obtained one-dimensional BPNR and one-dimensional PNR have neat edges and clean surfaces, with a length of about 1 to 2 μm, a width of about 30 to 50 nm, and a thickness of about 0.5 to 3 nm.
[0126] The upper layer of the centrifuge tube clear liquid 2 cm away from the surface was sucked out with a pipette and dried to obtain a mixture of one-dimensional BPNR and one-dimensional PNR. The SEM photo of the mixture is shown in Figure 4 As shown, it can be seen that the one-dimensional BPNR and one-dimensional PNR in the mixture of the obtained one-dimensional BPNR and one-dimensional PNR have neat edges and clean surfaces, with a length of about 10 to 30 μm, a width of about 50 to 100 nm, and a thickness of about 0.5 to 10 nm. The selected area electron diffraction (SAED) photo of the transmission electron microscope is shown as follows Figure 5 As shown, the symmetrical diffraction spots indicate that its structure is a single crystal structure.
[0127] (D) transferring the one-dimensional BPNR or one-dimensional PNR obtained in step (C) as a channel of a field effect transistor to the surface of the graphene contact electrode in step (B), specifically comprising:
[0128] S11. Use a pipette to suck the upper clear liquid in the centrifuge tube 2 cm away from the surface and drop it onto the surface of the graphene contact electrode (i.e., the patterned graphene). During the dropping process, ensure that only one one-dimensional BPNR or one one-dimensional PNR is successfully transferred to the surfaces of two adjacent graphene contact electrodes (with both ends overlapping the surfaces of two adjacent graphene contact electrodes);
[0129] S12. Then quickly put it into a vacuum tube furnace and -5 The dried samples were heated at 40°C for 12 h under a vacuum degree of 0.04 Pa; the dried samples were cleaned with acetone and isopropanol to remove the organic solvent remaining on the surface of the samples;
[0130] (E) accurately locating the position where the one-dimensional BPNR or one-dimensional PNR contacts the graphene contact electrode through the positioning mark on the target substrate, and then making source and drain electrodes on the surface of the graphene contact electrode, respectively, specifically including:
[0131] S13. Use a scanning electron microscope (SEM) to observe the position where the one-dimensional BPNR or one-dimensional PNR contacts the graphene contact electrode; in this embodiment, it is observed that the width of the nanoribbon successfully transferred to the surface of the graphene contact electrode is 50nm, the length is 10μm, and the thickness is 1nm, that is, the channel in this embodiment is a one-dimensional BPNR channel (composed of a one-dimensional BPNR). It is also possible to use a microscope transfer platform dry method to directly select a one-dimensional BPNR of a target size for transfer.
[0132] S14. Spin-coat the electronic photoresist PMMA950K with a thickness of 1 μm on the surface of the one-dimensional BPNR and the surface of the graphene contact electrode, and dry it on a hot plate at 120°C for 90 seconds;
[0133] S15. Patterning source and drain electrodes on the graphene surface by electron beam lithography (EBL) process, developing in developer, soaking in deionized water for 90s and 60s respectively, and drying with nitrogen gas;
[0134] S16. Using a thermal evaporation process, 5 nm thick Cr + 45 nm thick Au is evaporated on the surface of the graphene contact electrode after the source and drain electrodes are patterned, wherein the metal Cr is used as a bonding layer between the metal Au and the graphene contact electrode; then, soaking in acetone for 1 hour, ultrasonically oscillating in an ultrasonic cleaning machine for 10 seconds until the Cr / Au outside the source and drain electrode patterns fall off, taking out, rinsing with isopropanol, and blowing dry with nitrogen to form source and drain electrodes;
[0135] (F) transferring a layer of boron nitride as a top gate electrode on the surface of the one-dimensional BPNR and on the surface of the graphene contact electrode that is not covered by the source and drain electrodes, specifically comprising:
[0136] S17. Use blue tape to mechanically peel off the BN block to obtain a mixture of single-layer, double-layer, triple-layer, and few-layer boron nitride, and transfer it to the surface of the PDMS substrate. Then, use a microscope transfer platform to press the single-layer BN (thickness of about 0.33 nm) on the PDMS substrate onto the surface of the one-dimensional BPNR channel and the graphene contact electrode that is not covered by the source and drain electrodes to form a top gate electrode;
[0137] S18. Place the above device at about 10 -5 Pa vacuum annealing at 200 ° C for 30 min to improve the contact between BPNR and graphene contact electrode, that is, to obtain the final one-dimensional BPNR top-gate field effect transistor prepared by liquid phase exfoliation and cascade centrifugation method. The side schematic diagram of the field effect transistor is shown in Figure 6 As shown. After testing, the switching ratio of the field effect transistor prepared in this embodiment is as high as 10 6 The room temperature mobility is as high as 960cm 2 V -1 s -1 .
[0138] Comparative Example 1
[0139] Same as Example 1, except that step S17 is omitted and the device obtained in step S16 is directly placed on a plate about 10 -5 After annealing at 200°C for 30 min under a vacuum of 1.5 Pa, a field effect transistor without a top gate electrode is finally obtained. The side schematic diagram is shown in FIG. Figure 7 As shown. After testing, the switching ratio of the field effect transistor prepared in this comparative example is 10 5 The room temperature mobility is 720Acm 2 V -1 s -1 .
[0140] Comparative Example 2
[0141] The same as Example 1, the only difference is that the material of the top gate electrode is replaced with Al2O3 (thickness is 0.33nm), and its side schematic diagram is as follows Figure 8 As shown. After testing, the switching ratio of the field effect transistor prepared in this comparative example is 10 5 The room temperature mobility is 860Acm 2 V -1 s -1 .
[0142] Comparative Example 3
[0143] Same as Example 1, except that the graphene contact electrode is omitted. Fig. 9 As shown. After testing, the switching ratio of the field effect transistor prepared in this comparative example is 10 5 The room temperature mobility is 600Acm 2 V -1 s -1 .
[0144] Comparative Example 4
[0145] The same as Example 1, except that the one-dimensional BPNR and / or one-dimensional PNR are prepared by centrifugation at a speed of 6000 r / min for 6 hours instead of using a cascade centrifugation method. The final channel width in this comparative example is 50 nm, the length is 10 μm, and the thickness is 1 nm. After testing, the switching ratio of the field effect transistor prepared in this comparative example is within the range of 10 3 The room temperature mobility is 550A cm 2 V -1 s -1 .
[0146] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A field effect transistor based on one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon, characterized in that: The invention comprises a target substrate, a graphene contact electrode, a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon channel, a source electrode, a drain electrode and a boron nitride top gate electrode which are arranged in sequence; the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon is prepared by liquid phase exfoliation and cascade centrifugation method.
2. The field effect transistor according to claim 1, characterized in that The one-dimensional black phosphorus nanobelt or one-dimensional phosphorene nanobelt channel has a thickness of 0.5 to 20 nm, a width of 1 to 300 nm, and a length of 500 nm to 900 μm.
3. The method for preparing a field effect transistor according to any one of claims 1 to 2, characterized in that: The following steps are involved: (A) preparing a positioning mark on a substrate to obtain a target substrate with the positioning mark; (B) transferring graphene to the surface of the target substrate with the positioning mark, and patterning the graphene to obtain a graphene contact electrode; (C) Using black phosphorus crystals as raw materials, one-dimensional black phosphorus nanoribbons or one-dimensional phosphorene nanoribbons are prepared by liquid phase exfoliation and cascade centrifugation method; (D) transferring the one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon as a channel of a field effect transistor to the surface of the graphene contact electrode; (E) accurately locating the position where the one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon contacts the graphene contact electrode through the positioning mark on the target substrate, and then making source and drain electrodes on the surface of the graphene contact electrode respectively; (F) A layer of boron nitride is transferred onto the surface of the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon and the surface of the graphene contact electrode that is not covered by the source and drain electrodes as a top gate electrode.
4. The preparation method according to claim 3, characterized in that: The step (A) specifically comprises: spin coating a photoresist with a thickness of 0.1 to 50 μm on the surface of the substrate, and drying at 100 to 150° C. for 1 to 10 minutes; using a patterned mask with a positioning function to ultraviolet-expose the surface of the substrate for 5 seconds to 10 minutes, developing, and drying; and using a thermal evaporation or electron beam evaporation process to evaporate a metal with a thickness of 20 to 300 nm on the surface of the substrate after ultraviolet exposure and development to obtain a target substrate with a positioning mark.
5. The preparation method according to claim 3, characterized in that: The step (B) specifically comprises: soaking the graphene in a 0.1-1 mol / L ammonium persulfate solution for 1-24 hours, rinsing with clean water and transferring the graphene to the surface of the target substrate with the positioning mark described in step (A), and drying at 20-60° C. for 2-24 hours to obtain a graphene layer; spin coating a 0.1-50 μm thick photoresist on the surface of the graphene layer, and drying at 100-150° C. for 1-10 minutes; using a patterned mask to ultraviolet-expose the surface of the graphene layer for 5 seconds to 10 minutes, developing, and drying; and etching the graphene layer after ultraviolet exposure and development with oxygen plasma or argon ion beam to pattern it to obtain a graphene contact electrode.
6. The preparation method according to claim 3, characterized in that: The step (C) specifically includes: mixing black phosphorus crystals and an organic solvent to obtain a mixed solution; ultrasonically treating the mixed solution for 1 to 12 hours to obtain a black phosphorus dispersion; centrifuging the black phosphorus dispersion at centrifugal speeds of 2000 r / min, 4000 r / min, 6000 r / min, 8000 r / min, 12000 r / min, and 14000 r / min for 1 hour each, and using a pipette to absorb the supernatant after centrifugation in the centrifuge tube to obtain a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon.
7. The preparation method according to claim 3, characterized in that: The step (D) specifically comprises: transferring a one-dimensional black phosphorus nanoribbon or a one-dimensional phosphorene nanoribbon to the surface of the graphene contact electrode; -3 ~10 -5 Pa vacuum and heat at 30-80°C for 2-24h.
8. The preparation method according to claim 3, characterized in that: The step (E) specifically comprises: observing the contact position of the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon with the graphene contact electrode by using a scanning electron microscope; spin coating an electron photoresist with a thickness of 0.5 to 10 μm on the surface of the one-dimensional black phosphorus nanoribbon or the one-dimensional phosphorene nanoribbon and the surface of the graphene contact electrode, and drying at 100 to 150° C. for 1 to 10 minutes; patterning the source and drain electrodes on the surface of the graphene contact electrode by electron beam lithography, developing, and drying; and evaporating a metal with a thickness of 30 to 100 nm on the surface of the graphene contact electrode after the source and drain electrodes are patterned to form source and drain electrodes.
9. The preparation method according to claim 8, characterized in that: The step (F) specifically comprises: mechanically exfoliating the boron nitride block to obtain a mixture of single-layer, double-layer, triple-layer and few-layer boron nitride, transferring the mixture to the surface of the PDMS substrate, and then using a microscope transfer platform to press the single-layer boron nitride on the surface of the PDMS substrate onto the surface of the one-dimensional black phosphorus nanoribbon or one-dimensional phosphorene nanoribbon channel and the graphene contact electrode that is not covered by the source and drain electrodes to form a top gate electrode; and then placing the mixture at 10 -3 ~10 -5 The field effect transistor is obtained by annealing at 100-200° C. for 30-300 min under a vacuum of 0.04 Pa.
Citation Information
Cited By
Triazinyl cyclic compound-based nanofiltration membrane, method for preparing the same, and use thereof